E46-306 · Casting & Forging · Sand Casting · ★★
The pattern draft angle was only 0.5° (should be 2°); when the pattern was drawn the mold cavity tore and sand fell away, leaving scabs 2mm deep on the casting surface.
[Mechanism] Too small a draft angle makes the drawing friction high; the mold is pulled beyond its green strength and spalls.
[Calculation] The drawing resistance rises roughly inversely as the draft angle decreases; at 0.5° the resistance is about 4 times that at 2°.
[Design gap] The draft angle was not set adequately for the draw height.
① Set the draft angle: determine it from the draw height by table, using a larger draft for deep cavities
② Apply a release agent: paint or spray the pattern surface to reduce friction
③ Draw evenly: use draw pins to draw the pattern steadily and vertically, avoiding skew
④ Check the mold cavity: after drawing, check for scuffs and loose sand, detecting problems early
⑤ Repair the cavity: repair minor scuffs with coating, and remake the mold if severe
⑥ Pattern design: set the draft angle per standard and mark it on the drawing
⑦ Draw verification: confirm the absence of scuffs by the cavity appearance
⑧ Standardize process: write the draft angle into the pattern drawing, controlling at the source
GB/T 6414-2017 Castings - Dimensional tolerances