E46-307 · Casting & Forging · Cast Steel Part · ★★★
A cast steel part developed hot tears at the edge of a chill; they were 30mm long, and magnetic particle inspection showed the cracks running along the chill boundary.
[Mechanism] Excessive chilling by the chill forms a hard shell, and the adjacent liquid-solid two-phase zone, with its low strength, is pulled apart.
[Calculation] The chill raises the local cooling rate severalfold; when the thermal stress exceeds the tensile strength, cracking occurs.
[Design gap] The chills were not filleted and did not fit the mold surface uniformly.
① Fillet the chills: round the chill edges to avoid sharp-corner chilling
② Fit the mold surface: make the chill fit the mold surface with no gap to ensure uniform heat removal
③ Control the chilling: choose the chill thickness by wall thickness, avoiding excessive chilling
④ Surface treatment: keep the chill surface rust-free and dry, avoiding rust and moisture pickup
⑤ Crack check: magnetic particle inspect the chill boundary, detecting problems early
⑥ Slow-cooling measures: wrap the chill in asbestos when necessary to reduce chilling
⑦ Crack verification: confirm the absence of cracks by inspection
⑧ Standardize process: write the chill specification into the process drawing, controlling at the source
GB/T 11352-2009 Cast carbon steel castings for general engineering use