E46-308 · Casting & Forging · Sand Casting · ★★
Dense porosity appeared on the upper part of the casting, 1 to 3mm in diameter and covering about 8% of the surface area; the holes were exposed after machining.
[Mechanism] Pouring too fast makes the stream splash and entrain gas, which is trapped by solidification before it can rise out.
[Calculation] The entrained gas increases with the square of the pouring speed; keeping the speed below the critical value lets the gas rise out.
[Design gap] The gating system was not designed to control flow and vent gas.
① Control the pouring speed: set the flow rate by part weight so the stream fills the mold steadily
② Provide overflow and venting: fit overflow and vents at the pouring cup to discharge entrained gas
③ Use a filter: place a ceramic filter in the runner to steady the flow and trap slag
④ Reduce the drop: reduce the drop from the ladle nozzle to the sprue to cut splashing
⑤ Porosity check: magnetic particle inspect or X-ray the machined surface for holes, detecting problems early
⑥ Adjust the process: use bottom pouring or step gating when necessary
⑦ Porosity verification: confirm compliance by nondestructive testing
⑧ Standardize process: write the pouring speed into the process card, controlling at the source
GB/T 9438-2013 Aluminum-alloy castings