E46-309 · Casting & Forging · Cast Steel Part · ★★★
A cast steel part leaked at the chaplets inside the cavity; sectioning revealed an oxidized layer between the chaplet and the iron that had not fused, and the hydraulic test leaked.
[Mechanism] The chaplet surface is oxidized or insufficiently preheated, so the iron fails to fuse with it metallurgically and forms an isolating layer.
[Calculation] A large temperature difference between the chaplet and the iron lets the interface oxide layer hinder fusion; the chaplet temperature must approach that of the iron.
[Design gap] The chaplets were set without rust removal and preheating.
① Remove rust from chaplets: grind the chaplet surface before setting to remove scale
② Preheat the chaplets: preheat to above 120℃ to remove moisture
③ Choose a matching material: use a chaplet material close to that of the casting to aid fusion
④ Fix securely: make the chaplet support points firm so they don't shift during pouring
⑤ Leak check: run a hydraulic or airtightness test on the casting, detecting problems early
⑥ Sectional sampling: section critical parts to check the fusion condition
⑦ Fusion verification: confirm the absence of leaks by testing
⑧ Standardize process: write the chaplet handling requirements into the work instruction, controlling at the source
GB/T 11352-2009 Cast carbon steel castings for general engineering use