E46-312 · Casting & Forging · Gray Iron Casting · ★★
A gray iron casting showed type D undercooled graphite (should be type A flake); strength dropped about 20%, and the fracture appeared mottled.
[Mechanism] Too-rapid cooling or a low carbon equivalent makes austenite precipitate ahead of the eutectic, and the graphite grows as fine, curved type D undercooled graphite.
[Calculation] A carbon equivalent below 3.6% or a cooling rate above the critical value promotes undercooled graphite, and strength falls accordingly.
[Design gap] The carbon equivalent and the cooling rate tied to wall thickness were not checked.
① Adjust the carbon equivalent: set the carbon equivalent to 3.8 to 4.2 by wall thickness to keep type A graphite
② Control the cooling rate: smooth out wall-thickness transitions to avoid localized chilling
③ Inoculation: inoculate with ferrosilicon before pouring to promote type A graphite
④ Composition check: check the furnace-side rapid carbon and silicon analysis
⑤ Metallographic check: section the part and check the graphite morphology, detecting problems early
⑥ Strength check: measure the tensile strength to confirm compliance
⑦ Graphite verification: confirm type A predominates by metallography
⑧ Standardize process: write the carbon equivalent into the charge sheet, controlling at the source
GB/T 9439-2010 Grey cast iron castings