Knowledge Base › Process and Assembly Error Case Study › Oxide Inclusions in Aluminum Alloy

Oxide Inclusions in Aluminum Alloy

E46-313 · Casting & Forging · Aluminum Alloy Casting · ★★★

Problem Description

An aluminum alloy casting had oxide slag inclusions; X-ray showed a 10mm-long stringer inclusion, and after machining the slag was exposed on the surface, causing leaks in the airtightness test.

Root Cause

[Mechanism] Al2O3 oxide films from melting and pouring are not fully removed and are drawn into the mold cavity, forming hard, brittle inclusions.
[Calculation] Oxide films are entrained with stirring and pouring drop; incomplete degassing and deslagging raises the volume fraction of inclusions.
[Design gap] No refining and filtration steps were provided.

Corrective Solution

① Refine the melt: use rotary inert-gas injection to remove gas and slag
② Provide filtration: place a ceramic foam filter in the runner to trap slag
③ Control the drop: reduce the transfer-ladle drop to limit oxidation
④ Clean the charge: remove oil, rust, and scale from the charge before melting
⑤ Inclusion check: use X-ray or sectioning to check for slag inclusions, detecting problems early
⑥ Airtightness test: run a leak test to confirm
⑦ Inclusion verification: confirm the absence of stringer slag by X-ray
⑧ Standardize process: write the refining and filtration into the process card, controlling at the source

Checklist

Reference

GB/T 9438-2013 Aluminum-alloy castings

Related model download:Understood the principle and ready to try?Go to MOULDL to download related 3D models and CAD drawings for free »