E46-315 · Casting & Forging · Cast Steel Valve Body · ★★★
A cast steel valve body revealed shrinkage porosity after the sealing surface was machined; it leaked in the pressure test, and the whole batch had to be reworked.
[Mechanism] The shrinkage porosity lies beneath the machining allowance and is exposed once rough machining removes the allowance.
[Calculation] When the machining allowance is less than the depth at which the porosity lies, it is bound to be exposed; the hot-spot feeding must be checked against the allowance.
[Design gap] Enough machining allowance was not reserved and feeding was not checked.
① Check feeding: size the riser by the hot-spot modulus to ensure soundness
② Leave allowance: leave enough allowance on the machined surface to avoid the porosity layer
③ Flaw-detect up front: ultrasonic-inspect the machined surface before rough machining
④ Adjust the process: change the pouring position when necessary so the machined surface faces up
⑤ Leak test: run a pressure test after machining, detecting problems early
⑥ Rework and weld repair: clean the exposed porosity, weld-repair it, and re-inspect
⑦ Soundness verification: confirm the absence of leaks by pressure test
⑧ Standardize process: write the allowance and riser into the process drawing, controlling at the source
GB/T 11352-2009 Cast carbon steel castings for general engineering use