Knowledge Base › Process and Assembly Error Case Study › Sand Inclusion Scab

Sand Inclusion Scab

E46-317 · Casting & Forging · Plate Casting · ★★

Problem Description

A plate-type casting had a sand inclusion scab on the upper surface; the cavity beneath the scab was 3mm deep, exposing bare iron after cleaning.

Root Cause

[Mechanism] The high-temperature iron expands and heaves or delaminates the surface sand of the mold cavity; the iron penetrates and forms a scab.
[Calculation] The expansion increases with the sand's thermal expansion rate and heating rate; once it exceeds the bond strength, delamination occurs.
[Design gap] Low-expansion sand or coating protection was not used.

Corrective Solution

① Use low-expansion sand: choose low-expansion silica sand or add zircon flour
② Apply a coating: brush a refractory coating on the mold cavity to isolate the iron
③ Control temperature: lower the pouring temperature appropriately to reduce expansion
④ Add sawdust: add a small amount of sawdust to the molding sand to cushion expansion
⑤ Scab check: open the flask and check the upper surface, detecting problems early
⑥ Clean and repair: root out and weld-repair the scabbed area
⑦ Scab verification: confirm the absence of delamination by appearance
⑧ Standardize process: write the molding sand mix into the work instruction, controlling at the source

Checklist

Reference

GB/T 9442-2010 Silica Sand for Foundry Use

Related model download:Understood the principle and ready to try?Go to MOULDL to download related 3D models and CAD drawings for free »