E46-318 · Casting & Forging · Thin-Wall Gray Iron Casting · ★★
White iron cementite formed in the thin-wall sections of a gray iron casting; the hardness exceeded HB300, making machining impossible.
[Mechanism] Rapid cooling of thin walls makes the eutectic transform via the metastable system instead of the graphite system, precipitating cementite and forming white iron.
[Calculation] A wall thickness below the critical value or a low carbon equivalent produces white iron; a cooling rate above the critical value promotes cementite.
[Design gap] No inoculation or charge adjustment was made for thin-wall parts.
① Raise the carbon equivalent: use a high carbon equivalent for thin-wall parts to prevent white iron
② Inoculate before pouring: add ferrosilicon inoculation to promote graphitization
③ Control wall thickness: avoid excessively thin sections in design or thicken them
④ Reduce the cooling rate: lower the molding sand moisture or add insulation for slow cooling
⑤ Hardness check: measure the hardness at the thin-wall sections, detecting problems early
⑥ Annealing: graphitizing-anneal parts that have already chilled
⑦ White iron verification: confirm machinability by hardness
⑧ Standardize process: write the carbon equivalent and inoculation into the charge sheet, controlling at the source
GB/T 9439-2010 Grey cast iron castings