Knowledge Base › Process and Assembly Error Case Study › Die Casting Gas Porosity Causing Leakage

Die Casting Gas Porosity Causing Leakage

E46-321 · Casting & Forging · Die Casting · ★★★

Problem Description

A die casting had internal gas porosity; X-ray showed clusters of 2mm-diameter holes that were exposed after machining, causing leaks in the airtightness test.

Root Cause

[Mechanism] Cavity gas or vapors from the release agent are not fully vented and are drawn in and trapped by the high-speed metal.
[Calculation] The amount of entrained gas increases with injection velocity; insufficient vent area raises the cavity back pressure.
[Design gap] Adequate venting and release-agent control were not provided.

Corrective Solution

① Provide venting: cut vent grooves in the parting surface and inserts to fully vent the cavity
② Control the release agent: spray an appropriate amount to avoid excess gas accumulation
③ Optimize velocity: use a slow-fast-slow injection profile to reduce gas entrainment
④ Uniform die temperature: control the die temperature so the gas vents easily
⑤ Porosity check: X-ray or inspect the machined surface for holes, detecting problems early
⑥ Airtightness test: run a leak test to confirm
⑦ Porosity verification: confirm the absence of out-of-limit holes by X-ray
⑧ Standardize process: write the die casting parameters into the process card, controlling at the source

Checklist

Reference

GB/T 15114-2009 Aluminum Alloy Die Castings

Related model download:Understood the principle and ready to try?Go to MOULDL to download related 3D models and CAD drawings for free »