E46-322 · Casting & Forging · 40Cr Forging · ★★★
A 40Cr forging had a final-forging temperature of only 720℃ (should be ≥800℃); cracks formed along the deformation direction after forging, with a length of 15mm.
[Mechanism] At low temperature the metal has poor plasticity and high deformation resistance; cracking occurs once the fracture strength is exceeded.
[Calculation] Final forging below the recrystallization temperature accumulates work hardening, and cracks increase as the temperature falls.
[Design gap] The lower limit of the final-forging temperature was not controlled.
① Control the final-forging temperature: keep the final forging above the specification's lower limit
② Temperature monitoring: monitor in real time with infrared thermometry
③ Reheat: if the temperature is insufficient, return the part to the furnace, reheat, and forge again
④ Control deformation: reduce the single-pass reduction in the low-temperature stage
⑤ Crack check: magnetic particle inspect after forging, detecting problems early
⑥ Slow cooling: cool slowly after forging to reduce stress
⑦ Crack verification: confirm the absence of cracks by inspection
⑧ Standardize process: write the final-forging temperature into the process card, controlling at the source
GB/T 12361-2016 Steel die forgings - Process