E46-324 · Casting & Forging · Open-Die Forging · ★★★
During open-die drawing out the feed was too large; longitudinal cracks and folds formed inside the forging, and ultrasonic inspection revealed laminations.
[Mechanism] A feed ratio (feed divided by anvil width) that is too large puts the core in tension, and the forging is not fully worked through, producing internal defects.
[Calculation] The feed ratio should be 0.5 to 0.8; above 1.0 the core tensile stress exceeds the plasticity and causes cracking.
[Design gap] The matching of feed to anvil width was not specified.
① Control the feed ratio: set the feed to 0.5 to 0.8 times the anvil width
② Choose the anvil width: select a flat anvil wide enough for the blank diameter
③ Turn during forging: turn the part each pass to ensure the core is fully worked through
④ Control deformation: keep the single-pass reduction moderate
⑤ Internal check: ultrasonic-inspect for laminations after forging, detecting problems early
⑥ Grind out defects: grind the surface cracks
⑦ Work-through verification: confirm the absence of laminations by ultrasonic inspection
⑧ Standardize process: write the feed ratio into the forging card, controlling at the source
GB/T 15826-1995 Steel open-die forgings on hammers - Process