E46-325 · Casting & Forging · Die Forging · ★★
A die forging had a 1.8mm mismatch between the upper and lower dies; the flash was offset to one side, and after machining one side had insufficient allowance and showed bare metal.
[Mechanism] Excessive guide clearance in the die forging hammer or press, or a misaligned die, causes relative mismatch at the parting line.
[Calculation] The mismatch equals the sum of the guide clearance and the installation error; exceeding half the allowance causes bare metal.
[Design gap] Die alignment and guide accuracy were not controlled.
① Align the die: after mounting, strike a sample part to true up the parting line
② Control the guides: check the machine guide clearance and repair it if out of tolerance
③ Set the allowance: leave enough machining allowance for possible mismatch
④ First-article check: scribe the first article to check the mismatch, detecting problems early
⑤ Allowance re-measurement: measure the allowance distribution before machining
⑥ Die inspection and maintenance: periodically check the die locating keys
⑦ Mismatch verification: confirm the mismatch is ≤0.5mm by scribing
⑧ Standardize process: write the die alignment requirements into the work instruction, controlling at the source
GB/T 12362-2016 Steel die forgings - Tolerances