Knowledge Base › Process and Assembly Error Case Study › Graphite Flotation in Ductile Iron

Graphite Flotation in Ductile Iron

E46-342 · Casting & Forging · Heavy Ductile Iron Casting · ★★

Problem Description

On a thick, heavy ductile iron casting the top surface had a graphite flotation layer 3mm thick with low hardness; machining exposed porosity.

Root Cause

[Mechanism] An excessively high carbon equivalent or a high pouring temperature makes graphite float and collect at the surface.
[Calculation] A carbon equivalent above 4.6% or high superheat gives the graphite enough buoyancy, and the flotation layer grows with section thickness.
[Design gap] The carbon equivalent and pouring temperature were not controlled.

Corrective Solution

① Control carbon equivalent: use the middle of the range for heavy castings to prevent flotation
② Control pouring temperature: avoid pouring with excessive temperature or superheat
③ Use chills: place chills on the top surface to suppress flotation
④ Rework risers: optimize the riser so graphite collects there
⑤ Check for flotation: inspect the machined surface for a graphite layer, detecting problems early
⑥ Performance check: measure surface hardness
⑦ Flotation verification: confirm the absence of graphite accumulation by microstructure
⑧ Standardize process: write the carbon equivalent into the charge sheet, controlling at the source

Checklist

Reference

GB/T 1348-2009 Spheroidal graphite iron castings