E46-343 · Casting & Forging · Steel Casting · ★★★
Two chills on a steel casting were spaced too far apart, leaving the central hot spot unchilled; a shrinkage cavity 25mm deep was exposed during machining.
[Mechanism] Chills spaced too sparsely leave the middle region solidifying last with no feeding, forming shrinkage cavities.
[Calculation] When the chill spacing exceeds the effective chilling range, the middle becomes a hot spot and the cavity grows with the spacing.
[Design gap] The chill spacing was not verified.
① Denser chills: space chills according to the chilling range so that no isolated hot spot remains
② Verify spacing: keep the chill spacing below the effective chilling diameter
③ Match risers: supplement the spaces between chills with risers for feeding
④ Establish sequence: form directional solidification from the chills toward the riser
⑤ Check for cavities: ultrasonic inspect after rough machining, detecting problems early
⑥ Test block verification: check soundness with a cast-on test block
⑦ Cavity verification: confirm the absence of cavities by nondestructive testing
⑧ Standardize process: write the chill layout into the process drawing, controlling at the source
GB/T 11352-2009 Cast carbon steel castings for general engineering use