Knowledge Base › Process and Assembly Error Case Study › Failure to Dehydrogenize After Forging Causing Flakes

Failure to Dehydrogenize After Forging Causing Flakes

E46-348 · Casting & Forging · Large Alloy Steel Forging · ★★★

Problem Description

After a large alloy steel forging was left standing, internal flakes appeared; ultrasonic inspection revealed hairline defects and toughness dropped sharply.

Root Cause

[Mechanism] Hydrogen in the steel does not diffuse out fully and collects on cooling into flakes, i.e. hydrogen-induced cracks.
[Calculation] Hydrogen content and cooling rate determine flaking; insufficient slow-cooling dehydrogenization leaves hydrogen to collect.
[Design gap] No isothermal dehydrogenization treatment was performed after forging.

Corrective Solution

① Dehydrogenization: after forging, slow-cool isothermally so hydrogen diffuses out fully
② Control hydrogen in melting: control hydrogen during melting to reduce the source
③ Slow-cooling specification: set the slow-cooling curve according to section thickness
④ Ultrasonic inspection: inspect for flakes after forging and after standing
⑤ Hydrogen check: measure hydrogen content when necessary
⑥ Reprocess: re-dehydrogenize parts that already show flakes
⑦ Flake verification: confirm the absence of hairlines by ultrasonic inspection
⑧ Standardize process: write the dehydrogenization specification into the process card, controlling at the source

Checklist

Reference

JB/T 5073-1991 Heat treatment of forgings