E46-351 · Surface Treatment & Coating · Steel Structure Member · ★
After spraying, the coating on a steel structure peeled off in sheets at edges and welds; the cross-cut adhesion was grade 0 (should be grade 1) and oily residue on the surface felt tacky to the touch.
[Mechanism] Incomplete degreasing leaves an oil film barrier that sharply reduces the bond at the coating/substrate interface.
[Calculation] A residual oil film only about 1μm thick can cut adhesion by 60%, causing cross-cut peeling.
[Design gap] The degreaser was not selected according to the soil type, and temperature and time were not controlled.
① Choose degreaser: select an alkaline or solvent degreaser according to the soil type to ensure cleaning power
② Control temperature and time: hold the degreasing bath at 60℃ for 10 min to fully emulsify the soil
③ Add rinsing: rinse in two counterflow stages after degreasing to remove all residue
④ Check the surface: use the water-break test to check for a continuous water film, detecting oil early
⑤ Degrease and respray: re-degrease oily areas before coating to restore adhesion
⑥ Control oil sources: prevent recontamination by hand sweat and oil between operations to stay clean
⑦ Adhesion verification: confirm grade 1 by the cross-cut test, verified by data
⑧ Standardize process: write the degreasing parameters into the pretreatment process card, controlling at the source
GB/T 8923.1-2011 Preparation of steel substrates before application of paints