E46-352 · Surface Treatment & Coating · Steel Plate Member · ★
After sandblasting and coating, a steel plate showed blistering and peeling along blast pits after 6 months; the surface roughness Ra was only 12μm (should be 40-70μm), so the anchor pattern was too shallow.
[Mechanism] Low blasting pressure and fine abrasive produce a shallow anchor pattern, giving insufficient mechanical keying of the coating.
[Calculation] Below Ra 40μm the keying area drops by about 50%, reducing adhesion.
[Design gap] No matching of blasting pressure to abrasive particle size was specified.
① Raise pressure: increase blasting pressure to 0.6 MPa for stronger impact
② Choose abrasive: use G25 chilled iron grit or copper slag grit to ensure particle size
③ Control distance and angle: hold the nozzle 150 mm away at 70° and sweep uniformly
④ Check roughness: use the replica tape method to measure Ra 40-70μm, detecting problems early
⑤ Re-blast: re-blast deficient areas to a compliant anchor pattern to restore keying
⑥ Control abrasive: sieve the abrasive periodically to remove fines and keep it sharp
⑦ Roughness verification: confirm compliance with replica tape, verified by data
⑧ Standardize process: write the blasting parameters into the surface preparation specification, controlling at the source
GB/T 8923.1-2011 Preparation of steel substrates before application of paints