E46-354 · Surface Treatment & Coating · Outdoor Steel Structure · ★★
Eight months after coating, an outdoor steel structure showed rust again at the welds; the measured dry film thickness was only 80μm (should be 160μm), with both missed areas and an over-thin single coat.
[Mechanism] An over-thin single coat plus missed areas leave the total film thickness insufficient, sharply cutting the barrier life.
[Calculation] Halving the film thickness cuts the corrosion life to about 1/4; 80μm gives insufficient life.
[Design gap] Film thickness was not controlled per coat and in total by layers.
① Layered spraying: apply three coats, each about 60μm, to build up the total
② Control gun technique: hold the gun 200 mm from the work and traverse uniformly to avoid missed areas
③ Wet film measurement: measure the wet film of each coat to keep it even
④ Check dry film: use a magnetic thickness gauge to verify a total of 160μm, detecting problems early
⑤ Touch up: respray thin areas to specification to restore the barrier
⑥ Control the environment: apply below 85% humidity to prevent blushing
⑦ Film thickness verification: confirm the total thickness meets specification with a gauge, verified by data
⑧ Standardize process: write the film thickness requirements into the coating procedure, controlling at the source
GB/T 30790.1-2014 Paints and varnishes - Protective coating systems