Knowledge Base › Process and Assembly Error Case Study › Excessive Electrophoretic Voltage Causing Pinholes and Exposed Substrate

Excessive Electrophoretic Voltage Causing Pinholes and Exposed Substrate

E46-356 · Surface Treatment & Coating · Electrophoretic-Coated Part · ★★

Problem Description

After cathodic electrodeposition the film was densely covered with pinholes exposing the substrate; the voltage was 280V (should be 200V), causing localized breakdown.

Root Cause

[Mechanism] Excessive voltage intensifies electrolysis and breaks the film down into pinholes.
[Calculation] Above 220V the pinhole rate rises sharply; at 280V large areas are left exposed.
[Design gap] Stepwise voltage ramp-up was not used to limit the peak voltage.

Corrective Solution

① Stepwise ramp-up: ramp up in 60-120-180V steps to limit the peak
② Control voltage: keep the peak below 200V to prevent breakdown
③ Control time: 3 min of electrodeposition for full film formation
④ Check pinholes: section a sample to inspect for pinholes, detecting problems early
⑤ Re-coat: sand and re-deposit pinhole-affected parts to restore coverage
⑥ Control the bath: stabilize solids and pH to prevent anomalies
⑦ Film thickness verification: confirm even coverage with no exposed substrate using a thickness gauge, verified by data
⑧ Standardize process: write the voltage curve into the electrocoating procedure, controlling at the source

Checklist

Reference

GB/T 13492-1992 Automotive topcoats in various colors