E46-365 · Surface Treatment & Coating · Hydraulic cylinder · ★★★
The hydraulic cylinder cracked in service after hard chrome plating; the chrome layer was 120μm thick (should be 60μm) and the substrate was hardened, so stress caused the cracking.
[Mechanism] The chrome layer is too thick and hard-brittle, and it deforms out of step with the substrate, so it stress-cracks.
[Calculation] Beyond 80μm the internal stress of the chrome layer surges and cracks initiate.
[Design gap] Chrome thickness and substrate pretreatment were not controlled.
① Control chrome thickness: keep hard chrome thickness at 40-60μm to reduce stress
② Pre-treatment: stress-relief anneal the substrate first to reduce residual stress
③ Control current: plate with uniform current to prevent local thickening and keep the layer even
④ Crack check: use magnetic-particle inspection to find chrome-layer cracks and detect problems early
⑤ Re-plate: strip the chrome from cracked parts and re-plate to restore integrity
⑥ Control the substrate: keep substrate hardness suitable for bonding to prevent spalling
⑦ Thickness verification: confirm compliance by thickness measurement, confirmed by data
⑧ Standardize process: write chrome thickness into the chrome-plating process, controlling at the source
GB/T 11379-2008 Metallic coatings - Electrodeposited coatings of chromium for engineering purposes