E46-370 · Surface Treatment & Coating · Dacromet fastener · ★★
The Dacromet part showed red rust after 480h of salt spray (should be 720h); the coating was thin and under-sintered, so protection was insufficient.
[Mechanism] A thin coating and insufficient sintering leave many pores in the coating, reducing corrosion resistance.
[Calculation] Dacromet should be 8μm on both sides with adequate sintering; if thin, salt spray performance drops.
[Design gap] The number of coating passes and the sintering curve were not controlled.
① Control passes: use two dip-spin passes to ensure film thickness and adequate protection
② Control sintering: sinter at 320℃ for sufficient time to reduce porosity
③ Clean pretreatment: derust cleanly before coating to ensure bonding
④ Film-thickness check: use thickness measurement to check even thickness and detect problems early
⑤ Re-coat: re-coat thin parts and re-sinter to restore corrosion resistance
⑥ Control the bath ratio: keep the coating solution's solids content steady to prevent thin coatings
⑦ Salt-spray verification: confirm absence of red rust by salt spray, confirmed by data
⑧ Standardize process: write the number of passes and sintering into the Dacromet specification, controlling at the source
GB/T 18684-2002 Zinc-chromium coatings - Technical requirements