E46-371 · Surface Treatment & Coating · Steel plate component · ★
The steel plate developed yellow rust again over the weekend after blasting; more than 4 hours passed without painting and the activated surface rusted again.
[Mechanism] After blasting the activated surface absorbs moisture and oxidizes, so rust returns if painting is delayed.
[Calculation] At 70% relative humidity, rust returns after more than 4 hours and the anchor pattern is lost.
[Design gap] The interval between blasting and painting was not limited.
① Limit the interval: paint within 4 hours of blasting to prevent rust recurrence
② Control the environment: shorten the interval or dehumidify on humid days to preserve the active surface
③ Re-blast: re-blast rusted parts before painting to restore the anchor pattern
④ Interval check: check the surface for absence of rust to detect problems early
⑤ Paint quickly: apply shop primer to activated surfaces first to ensure sealing
⑥ Batch by time: blast in batches according to painting capacity to prevent backlog
⑦ Surface verification: confirm absence of rust by visual inspection, confirmed by data
⑦ Standardize process: write the interval into surface treatment, controlling at the source
GB/T 8923.1-2011 Preparation of steel substrates before application of paints