E46-380 · Surface Treatment & Coating · Heavy-coated steel structure · ★★
The heavy-coated part's film cracked after drying; the total film thickness exceeded 400μm (should be ≤250μm) and internal stress was high.
[Mechanism] Applying a heavy coat in one pass makes internal stress exceed the coating's strength, causing cracking.
[Calculation] Above 250μm the stress rises sharply, and above 400μm it cracks.
[Design gap] The total thickness was not controlled by layering.
① Control in layers: apply multiple coats to keep the total thickness ≤250μm and reduce stress
② Control each coat: keep a single coat below 120μm to prevent cracking
③ Choose high-build: use a high-build type to prevent cracking and preserve toughness
④ Crack check: check the film for absence of cracks to detect problems early
⑤ Re-coat: sand and re-layer cracked parts to restore integrity
⑥ Control the environment: apply at a suitable temperature to prevent fast drying and reduce stress
⑦ Film-thickness verification: confirm compliance by thickness measurement, confirmed by data
⑧ Standardize process: write the total thickness into the coating process, controlling at the source
GB/T 30790.1-2014 Paints and varnishes - Protective coating systems