MOULDLKnowledge Base3D Model DownloadsMembership
中文版Model Store »
HomeModels
Table of contents

Lithium Battery Equipment (5 articles)

Knowledge Base Home

📐 Standard Data

🧮 Calculators

📖 Selection Guides

🏭 Material Grades

❓ Engineer FAQ

🗂 Quick-Reference Categories

❌ Error Case Studies

📚 Technical Articles

Knowledge Base › Lithium-Battery Equipment › 2026-10-11_10_Lithium Battery Tab Welding Cold-Weld Case Study_BST

Lithium battery tab ultrasonic welding cold-weld case: checking the horn knurling and parameters item by item

Summary

A battery plant had cold welds in ultrasonic metal welding of aluminum tabs to the cap plate, with a mean vertical pull-off force of 228N (standard ≥200N), a CPK of only 0.52, and a defect rate of about 6%. This article checks quantitative evidence item by item along five lines — horn knurling wear, welding parameter window, tab oxide layer, fixture clearance, and equipment rigidity — gives the horn dressing interval and improved parameter values, and includes a before-and-after comparison table, so that readers can use it to troubleshoot their own welding stations.

Body

Problem description

On a module line at a power battery plant, aluminum tabs (a 5-layer stack of 0.1mm aluminum foil) are ultrasonically metal-welded to a positive cap plate aluminum sheet; the horn is of the longitudinal-vibration type and the weld point size is 4mm×4mm. The process requires a vertical pull-off force ≥200N and a fracture that is cohesive failure of the material.

A July 2026 customer complaint: finished products showed tab open circuits after vibration testing. Sampling the welding station's products over 3 consecutive days and running a vertical pull-off test on each, 300 pieces in total, gave a mean tensile force of 228N with a standard deviation of 18N and a defect rate of 5.9% (about 6%) below 200N. Taking the one-sided specification of 200N, CPK=(228−200)/(3×18)=0.52, so the process capability is seriously insufficient.

Dissecting the cold-weld points: the cold welds were concentrated at the discharge-side edge of the horn knurling, accounting for about 60%; the fracture showed a silvery metallic luster but no material tearing, which is interface-separation-type cold welding, not a pull-apart after fusion. The first article of a new shift passed, and the defect rate began to rise after about 2 hours of continuous production.

Cause analysis

Check item by item in the order "from easy to measure to hard to dismantle, from external to internal causes":

Check 1: surface condition of the horn and the anvil.

The horn was removed and its knurl height measured under a toolmaker's microscope. A new horn has a knurl height of 0.08mm; this horn had produced about 80,000 points continuously and the measured knurl height was only0.03mm, a wear rate of 62.5%. Once the knurling is worn flat it can no longer pierce the oxide layer on the tab surface, the ultrasonic energy cannot be effectively transmitted into the workpiece, and the interface is only pressed together without welding. The working face of the anvil also showed aluminum-chip indentations and a bright band.

Conclusion: the horn knurling was worn beyond its service interval, and this is the main cause of the cold welds.

Check 2: welding parameter window.

The machine parameters were retrieved: amplitude set at 80%, welding pressure 0.35MPa, welding time 0.30s, with no trigger-force monitoring. Re-measured with a force sensor, the actual applied pressure fluctuated between 0.30~0.42MPa. The high amplitude caused the tab surface material to spatter and form a ring-shaped flash, while the central zone was in fact not fully fused.

Conclusion: the parameter window was too narrow and had no closed loop.

Check 3: tab material and surface oxide layer.

Samples were taken to measure the contact resistance of the tab surface: an aluminum tab left open in the workshop for 72 hours had a contact resistance of about 3.2mΩ, while a freshly cut tab had about 0.8mΩ. The thickened natural oxide film lowers the efficiency of frictional heat generation in ultrasonic welding. On site, incoming tabs are stored for an average of 48~72 hours before going on the line.

Conclusion: the thickened oxide layer aggravates the cold welds.

Check 4: fixture positioning and clearance.

A feeler gauge was used to measure the gap at the mating face between the tab and the cap plate, giving a reading of0.10~0.15mm, while the process requires ≤0.05mm. When a gap exists, the welding pressure is first used to flatten the gap, leaving insufficient effective forging time, and the cold welds mostly appear on the side with the poorer fit.

Conclusion: flattening and positioning were inadequate.

Check 5: equipment rigidity.

A dial indicator measured the vertical play of the horn holder at 50% applied pressure, giving 0.06mm and an excessive guide bushing clearance. The play causes part of the ultrasonic energy to be lost in the vertical direction.

Conclusion: a decline in equipment rigidity is a secondary cause.

Overall judgment: horn knurling wear is the main cause, the narrow parameter window is a secondary cause, the thickened oxide layer and fixture clearance are aggravating factors, and equipment rigidity is a background factor.

Improvement plan

Improvement 1: horn knurl dressing and life management.The horn dressing interval was changed from 'dress it when there are too many cold welds' to management by point count: dress the knurling with an oilstone once every 20,000 welds, and force replacement when the knurl-height wear exceeds 30% (i.e. below 0.056mm); run a pull test on the first article at the start of every shift to confirm. Clean aluminum chips from the anvil working face once every 8 hours.

Improvement 2: recalibrate the welding parameter window.After a parameter DOE on the tab, the settings were locked in: amplitude reduced from 80% to 65% (about 26μm), welding pressure raised to 0.42MPa with pressure closed-loop control, welding time 0.28s, and a trigger-force trigger mode added (ultrasound is emitted only when the pressure reaches 90%). Test coupons verified that the mean tensile force held steadily above 260N.

Improvement 3: control the tab oxide layer.Tabs must go on the line within 24 hours of cutting, and open workshop positions must be fitted with moisture-proof covers; add a plasma cleaning or alcohol wiping step before welding, keeping the contact resistance ≤1.0mΩ.

Improvement 4: fixture and flattening mechanism.Add a pneumatic flattening block beside the welding head to press the tab against the cap plate before welding, and recheck with a feeler gauge that the clearance is ≤0.05mm; change the locating stop block to a quick-change type and re-check it with a dial indicator after a model change.

Improvement 5: restore equipment rigidity.Replace the guide bushing of the horn holder, keeping the vertical play at 50% applied pressure within 0.02mm.

Implementation results

After the rework the line was tracked continuously for 2 months, with 20 pieces sampled per shift for a pull-off test; the key indicators compare as follows:

IndicatorBefore reworkAfter rework
Mean pull-off force228N262N
Pull-off force standard deviation18N12N
Process capability CPK0.521.72
Tensile defect rate (<200N)5.9%0.4%
Distribution of cold-weld locationsConcentrated at the discharge-side edge, 60%Evenly distributed
Horn knurl height0.03mm (62.5% wear)0.07~0.08mm (after dressing)
Amplitude/pressure/time80%/0.35MPa/0.30s65%/0.42MPa/0.28s
Tab storage time48~72h≤24h
Gap between the tab and the cap plate0.10~0.15mm≤0.05mm
Vertical play of the horn holder0.06mm≤0.02mm

After 2 months the machine was opened up to inspect the horn: the knurling was still clear, the flash was noticeably reduced, the mean tensile force held steady in the 255~270N range, and the CPK stayed above 1.6.

Result Verification and Pitfall Reminders

  1. For cold welds, check the horn knurling first — do not start by adjusting parameters. Once the knurling is worn flat, no amount of amplitude increase can transmit energy, so measure the knurl height first before anything else. It is advisable to measure it periodically with a toolmaker's microscope or a projector rather than judging by eye.
  2. Welding parameters need window verification — do not copy the equipment's default values. Run a three-level test coupon for each of the three variables (amplitude, pressure, time) per a DOE, plot the curves of mean tensile force and standard deviation, and pick the point with a high mean and a small standard deviation rather than looking at the mean alone.
  3. The fracture morphology must be included in inspection. If the tensile force is sufficient but the fracture is interface separation, long-term reliability will still suffer. Inspection should require the fracture to be cohesive tearing of the material; interface separation is judged suspicious even if the tensile force passes.
  4. Aluminum tab and copper tab processes cannot be used interchangeably. Aluminum tabs are more sensitive to a thick oxide film, so the cleaning step cannot be skipped; for copper tabs the focus is preventing the horn from picking up and transferring a copper layer.

Suggested Illustrations

If you are stuck on structure, browse the full-line 3D models in the 'MOULDL model library (mouldl model library)' (such as injection molding machines and pin-insertion machines, with parts lists); for data, double-check with the 'BST Technical Handbook' to be safer.

This article was compiled by Baist Technology (BST) as a reference for mechanical selection.

Related model download:Understood the principle and ready to try?Go to MOULDL to download related 3D models and CAD drawings for free »
MOULDL · Mechanical Engineering Knowledge Base · free self-study reference for machine designers, 3D CAD models at MOULDL