Welding method: CO2 gas-shielded welding
Base metal: Q235, plate thickness: 3mm
Welding current: 90A
Welding voltage: 18V
Wire diameter: φ0.8
Shielding gas flow: 15~20L/min
Use short-circuiting transfer or fine-droplet transfer.
Welding method: CO2 gas-shielded welding
Base metal: Q235, plate thickness: 5mm
Welding current: 130A
Welding voltage: 19V
Wire diameter: φ0.8
Shielding gas flow: 15~20L/min
Use short-circuiting transfer or fine-droplet transfer.
Welding method: CO2 gas-shielded welding
Base metal: Q235, plate thickness: 8mm
Welding current: 170A
Welding voltage: 20V
Wire diameter: φ1.0
Shielding gas flow: 15~20L/min
Use short-circuiting transfer or fine-droplet transfer.
Welding method: CO2 gas-shielded welding
Base metal: Q235, plate thickness: 10mm
Welding current: 200A
Welding voltage: 22V
Wire diameter: φ1.0
Shielding gas flow: 15~20L/min
Use short-circuiting transfer or fine-droplet transfer.
Welding method: CO2 gas-shielded welding
Base metal: Q235, plate thickness: 12mm
Welding current: 240A
Welding voltage: 23V
Wire diameter: φ1.2
Shielding gas flow: 15~20L/min
Use short-circuiting transfer or fine-droplet transfer.
Welding method: CO2 gas-shielded welding
Base metal: Q235, plate thickness: 16mm
Welding current: 280A
Welding voltage: 24V
Wire diameter: φ1.2
Shielding gas flow: 15~20L/min
Use short-circuiting transfer or fine-droplet transfer.
Welding method: CO2 gas-shielded welding
Base metal: Q235, plate thickness: 20mm
Welding current: 320A
Welding voltage: 26V
Wire diameter: φ1.2
Shielding gas flow: 15~20L/min
Use short-circuiting transfer or fine-droplet transfer.
Welding method: CO2 gas-shielded welding
Base metal: Q235, plate thickness: 25mm
Welding current: 360A
Welding voltage: 28V
Wire diameter: φ1.6
Shielding gas flow: 15~20L/min
Use short-circuiting transfer or fine-droplet transfer.
Welding method: CO2 gas-shielded welding
Base metal: 45 steel, plate thickness: 5mm
Welding current: 120A
Welding voltage: 19V
Wire diameter: φ0.8
Shielding gas flow: 15~20L/min
Use short-circuiting transfer or fine-droplet transfer.
Welding method: CO2 gas-shielded welding
Base metal: 45 steel, plate thickness: 10mm
Welding current: 180A
Welding voltage: 21V
Wire diameter: φ1.0
Shielding gas flow: 15~20L/min
Use short-circuiting transfer or fine-droplet transfer.
Welding method: CO2 gas-shielded welding
Base metal: 45 steel, plate thickness: 16mm
Welding current: 260A
Welding voltage: 24V
Wire diameter: φ1.2
Shielding gas flow: 15~20L/min
Use short-circuiting transfer or fine-droplet transfer.
Welding method: CO2 gas-shielded welding
Base metal: 45 steel, plate thickness: 20mm
Welding current: 300A
Welding voltage: 26V
Wire diameter: φ1.2
Shielding gas flow: 15~20L/min
Use short-circuiting transfer or fine-droplet transfer.
Welding method: CO2 gas-shielded welding
Base metal: 45 steel, plate thickness: 25mm
Welding current: 340A
Welding voltage: 28V
Wire diameter: φ1.6
Shielding gas flow: 15~20L/min
Use short-circuiting transfer or fine-droplet transfer.
Welding method: TIG tungsten inert gas welding (pure CO2 welding adds carbon and causes intergranular corrosion, so it is not suitable)
Base metal: 304 stainless steel, plate thickness: 3mm
Filler wire: ER308L (φ1.6)
Shielding gas: pure Ar, flow: 8~12L/min
Welding current: 80~110A
Welding voltage: 12~15V
Polarity: direct current electrode negative (DCEN)
Tungsten electrode: ceriated tungsten φ2.0
Purge the back side with shielding gas to prevent oxidation.
Use short-circuiting transfer or fine-droplet transfer.
Welding method: TIG tungsten inert gas welding (pure CO2 welding adds carbon and causes intergranular corrosion, so it is not suitable)
Base metal: 304 stainless steel, plate thickness: 5mm
Filler wire: ER308L (φ2.0)
Shielding gas: pure Ar, flow: 10~14L/min
Welding current: 110~150A
Welding voltage: 13~16V
Polarity: direct current electrode negative (DCEN)
Tungsten electrode: ceriated tungsten φ2.4
A V-groove (60°~70°) is recommended; purge the back side with shielding gas.
Use short-circuiting transfer or fine-droplet transfer.
Welding method: TIG tungsten inert gas welding (pure CO2 welding adds carbon and causes intergranular corrosion, so it is not suitable)
Base metal: 304 stainless steel, plate thickness: 8mm
Filler wire: ER308L (φ2.4)
Shielding gas: pure Ar, flow: 12~16L/min
Welding current: 150~190A
Welding voltage: 14~17V
Polarity: direct current electrode negative (DCEN)
Tungsten electrode: ceriated tungsten φ3.0
A V-groove (60°~70°) is required, with multi-pass welding and back-side gas purging.
Use short-circuiting transfer or fine-droplet transfer.
Welding method: TIG tungsten inert gas welding (pure CO2 welding adds carbon and causes intergranular corrosion, so it is not suitable)
Base metal: 304 stainless steel, plate thickness: 10mm
Filler wire: ER308L (φ2.4)
Shielding gas: pure Ar, flow: 12~16L/min
Welding current: 180~220A
Welding voltage: 15~18V
Polarity: direct current electrode negative (DCEN)
Tungsten electrode: ceriated tungsten φ3.0
A V-groove (60°~70°) is required, with multi-pass, multi-run welding and back-side gas purging.
Keep the interpass temperature ≤150℃ to prevent intergranular corrosion.
Use short-circuiting transfer or fine-droplet transfer.
Welding method: MIG metal inert gas welding (CO2 welding is prohibited; CO2 reacts violently with the aluminum weld pool and welding is impossible)
Base metal: aluminum alloy (6061/5052), plate thickness: 3mm
Filler wire: ER4043 (φ1.0) or ER5356 (φ1.0)
Shielding gas: pure Ar (argon), flow: 15~20L/min
Welding current: 110~140A
Welding voltage: 18~22V
Polarity: direct current electrode positive (DCEP)
The oxide film must be removed before welding (chemical cleaning or mechanical brushing).
Use spray transfer or pulsed transfer.
Welding method: MIG metal inert gas welding (CO2 welding is prohibited)
Base metal: aluminum alloy, plate thickness: 5mm
Filler wire: ER4043 (φ1.2) or ER5356 (φ1.2)
Shielding gas: pure Ar, flow: 18~22L/min
Welding current: 150~190A
Welding voltage: 20~24V
Polarity: direct current electrode positive (DCEP)
Remove the oxide film before welding. A V-groove is recommended (groove angle 60°~70°).
Use spray transfer or pulsed transfer.
Welding method: MIG metal inert gas welding (CO2 welding is prohibited)
Base metal: aluminum alloy, plate thickness: 8mm
Filler wire: ER4043 (φ1.6) or ER5356 (φ1.6)
Shielding gas: pure Ar, flow: 20~25L/min
Welding current: 190~240A
Welding voltage: 22~26V
Polarity: direct current electrode positive (DCEP)
A V-groove (60°~70°) is required, with multi-pass welding.
Remove the oxide film before welding and clean between passes.
Welding method: MIG metal inert gas welding (CO2 welding is prohibited)
Base metal: aluminum alloy, plate thickness: 10mm
Filler wire: ER4043 (φ1.6) or ER5356 (φ1.6)
Shielding gas: pure Ar, flow: 20~25L/min
Welding current: 230~280A
Welding voltage: 24~28V
Polarity: direct current electrode positive (DCEP)
A V-groove (60°~70°) is required, with multi-pass, multi-run welding.
Remove the oxide film before welding, clean between passes, and relieve stress after welding.
Other quick references in this series:Tolerances and FitsSurface RoughnessMaterial Heat TreatmentCasting DesignGeometric TolerancesDimensional chainWelded StructuresSheet Metal StructuresShaft System DesignSealing DesignMaterial SelectionHeat treatmentDatum LocationTolerancing principle