① High hardness HRC 62~68 (still HRC 60+ at 600℃)
② High strength and toughness (flexural σb=3~4GPa, high impact toughness)
③ Medium to low cutting speed (vc=20~50m/min on carbon steel)
④ Easy to grind and form (complex tools can be made)
⑤ Low cost
1. W18Cr4V (tungsten series)
C:0.7~0.8%, W:17.5~19%, Cr:3.8~4.4%, V:1.0~1.4%
General purpose, good wear resistance, slightly lower toughness
Heat treated hardness HRC 62~65
2. W6Mo5Cr4V2 (M2, molybdenum series)
C:0.8~0.9%, W:5.5~6.75%, Mo:4.5~5.5%, Cr:3.8~4.4%, V:1.75~2.2%
Better toughness than W18, finer and more uniform carbides
The most widely used
3. W6Mo5Cr4V2Al (extra hard type)
Contains aluminium, hardness HRC 67~69
Suited to high strength steel / stainless steel
4. W2Mo9Cr4VCo8 (M42, cobalt super hard)
HRC 67~70, the best red hardness
Suited to high temperature alloys / titanium alloys
Expensive
Quenching temperature: 1200~1280℃ (salt bath furnace)
Cooling: oil quench or martempering
Tempering: 560℃×3 times (1 hour each)
Final hardness HRC 62~67
1. Complex forming tools (twist drills / reamers / taps / hobs / gear shapers)
2. Low speed finishing
3. Machines with poor rigidity (high toughness, impact resistant)
4. Small batch production
5. Repair machining
High speed cutting (the hardness drops above 600℃)
High hardness workpieces (HRC>40)
Large batch production (short tool life)
Red hardness: HSS<600℃, carbide<900℃
Toughness: HSS>>carbide
Speed: HSS<50m/min, carbide>100m/min
Forming: HSS can be ground into complex shapes, carbide only simple shapes
By the workpiece material (internationally used):
P — steel (blue)
M — stainless steel (yellow)
K — cast iron (red)
N — non-ferrous metals (green)
S — super alloys / titanium (brown)
H — hardened materials (white)
By composition (China):
1. YG series (K class) — WC+Co
YG3X, YG6, YG6X, YG8, YG15
Co content 3~15%
Machining cast iron / non-ferrous / non-metal / hard materials
High toughness, impact resistant
2. YT series (P class) — WC+TiC+Co
YT5, YT14, YT15, YT30
TiC content 5~30%
Machining steel
Wear and red hardness high, low toughness
3. YW series (M class) — WC+TiC+TaC+Co
YW1, YW2, YW3
General purpose, machines both steel and cast iron
TaC improves toughness and thermal shock resistance
4. YN series — TiC based (cermet)
YN05, YN10
High hardness and wear resistance, low toughness
Suited to steel finishing
Carbide substrate + surface coating (2~15μm)
Coating materials:
TiN (gold, general purpose)
TiCN (grey violet, wear resistant)
TiAlN (purple black, high speed and heat resistant)
Al2O3 (black, ultra high temperature)
DLC (black, aluminium / non-ferrous)
nACO (nano multilayer)
Coating improves the life by 2~5 times
The permissible cutting speed rises by 30~50%
Rough turning steel: P10~P30 (YT5, YT14)
Finish turning steel: P05~P10 (YT30, YN10)
Turning cast iron: K10~K30 (YG6, YG8)
Turning stainless steel: M10~M30 (YW1, YW2)
Turning aluminium: N05~N20 (K10 uncoated)
Turning super alloys: S05~S20 (fine grain YG)
C45 steel turning, roughing
Select a P25 coated carbide insert
vc=180m/min, f=0.4mm/r, ap=3mm
Life about 30~45min (coated tool)
Hardness HRA 89~94 (HRC 74~82)
Red hardness <900℃ (up to 1100℃ with coating)
Flexural strength 1.2~2.5GPa
Low impact toughness (only 1/3 of HSS)
Low thermal expansion coefficient (4~6×10⁻⁶/℃)
Material: Al2O3 based or Si3N4 based
Characteristics:
① High hardness HRA 91~95
② Good red hardness (retains hardness below 1200℃)
③ Good chemical stability (not reactive)
④ Long wear life
⑤ Low toughness (prone to chipping)
⑥ Poor thermal shock resistance (cannot be coolant cooled)
Types:
1. Alumina based (Al2O3+TiC)
Brown / black
Finish turning of steel / cast iron
vc=200~500m/min
2. Silicon nitride based (Si3N4)
Grey
Better toughness, thermal shock resistant
High speed rough turning of cast iron / nickel alloys
vc=300~800m/min
3. Whisker toughened (Al2O3+SiC whiskers)
Significantly improved toughness
Suited to hardened steel / nickel alloys
Hardness HV 3500~4500 (second only to diamond)
Thermal stability <1400℃
Chemically inert (does not react with iron)
Suitable for:
① Hardened steel HRC 45~70 (turning instead of grinding)
② Nickel base super alloys
③ Hard cast iron (HS 65~80)
④ Sintered iron base alloys
Cutting speeds:
Hardened steel: vc=100~200m/min
Nickel alloys: vc=100~300m/min
PCBN (polycrystalline CBN) inserts: CBN content 50~95%
High CBN content: good toughness, machining cast iron
Low CBN content: machining hardened steel (finishing)
Hardness HV 6000~8000 (the hardest)
Thermal stability <700℃
Suitable for:
① Aluminium alloys (high silicon aluminium is best)
② Copper alloys
③ Engineering plastics / composites
④ Carbide
⑤ Ceramics
Cannot machine: ferrous materials (diamond is reactive with iron)
Cutting speeds:
Aluminium: vc=500~3000m/min
Copper: vc=300~1000m/min
HRC<30 workpiece: carbide
HRC 30~45: coated carbide / ceramic
HRC 45~65: CBN
HRC>65: CBN (roughing) / grinding
Non-ferrous metals: PCD
1. A machine with good rigidity (otherwise it chips)
2. A negative rake angle (increases the edge strength)
3. Choice of coolant or dry cutting (ceramic thermal shock)
4. Avoid impact (continuous cutting)
5. High cutting speed (low speed wears faster)
1. Increase the surface hardness (HV 2000~3500)
2. Reduce the friction coefficient (0.1~0.4)
3. Provide thermal insulation (lower substrate temperature)
4. Prevent diffusion (a chemical barrier)
5. Improve oxidation resistance
Effect: tool life improves by 2~10 times
Cutting speed rises by 30~100%
1. CVD (chemical vapour deposition)
Temperature: 800~1100℃
Coatings: TiN/TiCN/Al2O3/TiN multilayer
Thickness: 5~15μm
Suitable for: carbide inserts
Disadvantage: the high temperature reduces the substrate toughness
2. PVD (physical vapour deposition)
Temperature: 200~500℃
Coatings: TiN/TiCN/TiAlN/CrN/DLC
Thickness: 1~5μm
Suitable for: HSS / carbide
Advantages: the low temperature does not affect the substrate, complex shapes can be coated
3. MTCVD (medium temperature CVD)
Temperature: 700~900℃
Combines the advantages of CVD and PVD
Reduces substrate embrittlement
1. TiN (titanium nitride)
Golden yellow, HV 2200
General purpose coating, low friction coefficient
Use temperature <500℃
2. TiCN (titanium carbonitride)
Grey violet, HV 3000
Better wear resistance than TiN
Suited to steel machining
3. TiAlN (titanium aluminium nitride)
Purple black, HV 2800
High temperature oxidation resistance (800℃+)
First choice for high speed dry cutting
The Al2O3 oxide film protects it
4. Al2O3 (aluminium oxide)
Black, HV 2300
Excellent thermal insulation
High speed machining of cast iron / steel
5. DLC (diamond-like carbon)
Black, HV 3000+
Friction coefficient 0.1
Aluminium / non-ferrous / plastics
Cannot machine ferrous materials
6. nACo (nano multilayer)
Alternating TiAlN/CrN nano layers
Prevents crack propagation
The latest high performance coating
Steel at medium speed: TiN/TiCN
Steel at high speed: TiAlN/Al2O3
Cast iron: Al2O3
Aluminium: DLC
Stainless steel: TiAlN
Super alloys: TiAlN + lubrication
Single layer→multilayer→nano multilayer→gradient coating
Example: substrate/TiCN/TiAlN/Al2O3 (three layers)
Each layer plays a different role, the performance is better than a single layer
1. Abrasive
2. Grit
3. Bond
4. Hardness
5. Structure
1. Brown alumina A (Al2O3, contains TiO2)
Brown, good toughness
Grinding carbon steel / alloy steel / bronze
2. White alumina WA (pure Al2O3)
White, hard and brittle, good self-sharpening
Grinding hardened steel / high speed steel / tools
3. Chromium alumina PA (Al2O3+Cr2O3)
Rose red, tough abrasive
High precision grinding
4. Black silicon carbide C (SiC)
Black, harder than alumina, brittle
Grinding cast iron / brass / rubber / ceramics
5. Green silicon carbide GC (high purity SiC)
Green, very hard and brittle
Grinding carbide / gemstones / glass
6. Cubic boron nitride CBN
Grinding hardened steel / super alloys
7. Diamond D
Grinding carbide / ceramics / glass
Grit number = the mesh count of the screen (holes per inch of length)
Coarse: F12~F24 (rough grinding, deburring)
Medium: F30~F60 (general grinding)
Fine: F70~F180 (finish grinding)
Extra fine: F220~F600 (super finish grinding / lapping)
Selection principles:
Rough grinding: coarse grit (large allowance, high efficiency)
Finish grinding: fine grit (high accuracy, low roughness)
Soft materials: coarse grit (prevents clogging)
Hard materials: fine grit
1. Ceramic V — heat and corrosion resistant, brittle, general purpose
2. Resin B — high strength and elastic, high speed grinding
3. Rubber R — very elastic, centerless grinding / cut-off
4. Metal M — high strength, used for CBN / diamond
Refers to how easily the abrasive grains break away, not the hardness of the abrasive
Extra soft E-F
Soft G-H
Medium soft J-K
Medium L-M
Medium hard N-P
Hard Q-R
Extra hard S-T
Selection:
Hard materials: a soft wheel (the grains break away easily and stay sharp)
Soft materials: a hard wheel (the grains stay and do the grinding)
Finish grinding: a hard wheel
Rough grinding: a soft wheel
The volume ratio of the abrasive grains in the wheel
Dense 0~3, medium 4~6, open 7~12
Soft materials / thin walled parts: open (prevents clogging and distortion)
Precision grinding: dense
WA46K5V35
WA: white alumina
46: grit 46#
K: hardness K (medium soft)
5: structure number 5 (medium)
V: vitrified bond
35: maximum work line speed 35m/s
Normal: 30~35m/s
High speed grinding: 60~80m/s
Ultra high speed: >120m/s
CBN wheels can reach 80~120m/s
Diamond wheels 15~30m/s
Related quick references: Machining FundamentalsTool GeometryTurning ProcessMilling ProcessDrilling ProcessBoring ProcessGrinding ProcessMachining AllowanceProcess SequencingTypical ProcessesCNC ProgrammingFixture DesignSpecial Machining Processes