MOULDLKnowledge Base3D Model DownloadsMembership
中文版Model Store »
Knowledge Base › Machining Processes › Grinding Process
HomeModels
Table of contents

On this page

Knowledge Base Home

📐 Standard Data

🧮 Calculators

📖 Selection Guides

🏭 Material Grades

❓ Engineer FAQ

🗂 Quick-Reference Categories

❌ Error Case Studies

📚 Technical Articles

Machining Processes · Grinding Process (Quick Reference)

External Cylindrical Grinding Process and Parameters

【Classification of External Grinding】

1. plunge grinding (longitudinal feed, most common)

The workpiece rotates and moves longitudinally

The wheel feeds crosswise (the grinding depth)

2. cut-off grinding (infeed grinding)

The wheel is wider than the workpiece

Only a crosswise feed

High efficiency

3. deep grinding

A large depth of cut with a small feed

Removes the whole allowance in one pass

4. centerless grinding

The workpiece is not held between centers

Supported by the guide wheel and the work rest

Suited to small parts in large batches

【Grinding Motions】

1. Primary motion — the wheel rotates

vs = π·Ds·ns/1000 (m/s)

Ds — the wheel diameter

ns — the wheel speed

vs=30~35m/s (normal), 60~80m/s (high speed)

2. Peripheral feed — the workpiece rotates

vw = π·dw·nw/1000 (m/min)

vw=10~30m/min (roughing), 5~15m/min (finishing)

3. Longitudinal feed — the workpiece moves axially

fa = (0.2~0.8)Bs (mm/rev)

Bs — the wheel width

4. Crosswise feed (grinding depth)

fr = 0.005~0.05mm/double stroke

Rough grinding: 0.02~0.05mm

Finish grinding: 0.005~0.01mm

【Grinding Parameter Selection (C45 Steel)】

Wheel: WA46K5V35 (white alumina, grit 46, hardness K)

Rough grinding:

vs=30m/s, vw=20m/min, fa=0.5B, fr=0.03mm

Finish grinding:

vs=30m/s, vw=10m/min, fa=0.2B, fr=0.005mm

Spark-out grinding (no sparks):

fr=0, 2~3 passes

Eliminates the elastic recovery of the deformation

【Grinding Allowance】

Hardened steel:

Rough grinding 0.1~0.3mm

Finish grinding 0.02~0.1mm

Not hardened:

Rough grinding 0.2~0.5mm

Finish grinding 0.05~0.2mm

【Grinding Fluid】

Emulsion (common, good cooling)

Extreme pressure cutting oil (high accuracy)

Water based synthetic fluid (high speed grinding)

Flow: 10~50L/min

Pressure: 0.3~1MPa (normal)

3~10MPa (high pressure through-wheel coolant)

【Grinding Accuracy】

Dimensional accuracy IT5~IT6

Roundness 0.5~3μm

Cylindricity 1~5μm/300mm

Surface Ra0.4~0.8 (finish grinding)

Ra0.1~0.4 (precision grinding)

Ra0.025~0.1 (super finish grinding)

【Grinding Problems】

1. Burning

Cause: the grinding temperature is too high

Countermeasure: reduce the grinding depth / adequate cooling / a soft wheel

2. Cracking

Cause: quenching stress plus the grinding heat

Countermeasure: temper the workpiece / reduce the grinding depth / adequate cooling

3. Roundness error

Cause: poor center holes / an unbalanced workpiece

Countermeasure: repair the center holes / balance it

4. Cylindricity error

Cause: the machine guideways / wheel wear

Countermeasure: repair the guideways / dress the wheel

5. Surface waviness

Cause: vibration

Countermeasure: balance the wheel / damping

【Calculation Example】

External grinding D=40mm, hardened C45 steel

Rough grinding: vs=30m/s, ns=1000×30×1000/(π×400)=23874rpm? Not correct

Let the wheel Ds=400mm, ns=1430rpm

vs=π×400×1430/1000/60=30m/s ✓

vw=20m/min

nw=1000×20/(π×40)=159rpm

fa=0.5×50=25mm/rev

fr=0.03mm/double stroke

After finish grinding Ra=0.4μm, IT6

Internal Cylindrical Grinding and Surface Grinding

【Characteristics of Internal Grinding】

1. A small wheel diameter (<2/3 of the bore)

A low peripheral speed (limited by the spindle speed)

A high speed spindle is needed (electric / pneumatic)

2. A long slender wheel arbor

Poor rigidity, prone to vibration

3. A long contact arc

A large amount of grinding heat, difficult chip evacuation

4. Difficult measurement

The internal bore is inconvenient to measure

【Internal Grinding Parameters】

Wheel diameter Ds = (0.5~0.9)D bore

Wheel speed vs=10~25m/s (normal)

vs=25~45m/s (high speed electric spindle)

Workpiece speed vw=10~30m/min

Longitudinal feed fa=(0.3~0.7)Bs

Crosswise feed fr=0.002~0.02mm/double stroke

【Wheel Selection for Internal Grinding】

Small bores (D<10): WA80~120K~L

Medium bores (D=10~50): WA60~80J~K

Large bores (D>50): WA46~60G~J

【Internal Grinding Problems】

1. Bell mouth

Cause: the wheel overruns the end of the hole too much

Countermeasure: adjust the overrun

2. Taper

Cause: wheel wear / thermal deformation of the workpiece

Countermeasure: dress the wheel / adequate cooling

3. Poor roundness

Cause: chuck deformation / vibration of the wheel arbor

Countermeasure: reduce the clamping force / repair the wheel arbor

4. Surface burning

Cause: insufficient cooling

Countermeasure: increase the cooling / reduce the grinding depth

【Surface Grinding】

1. Peripheral grinding (the wheel circumference)

A small contact area, good heat dissipation, high accuracy

Magnetic chuck / rotary table

2. Face grinding (the wheel end face)

A large contact area, high efficiency, low accuracy

Suited to roughing

【Surface Grinding Parameters】

Wheel: WA36~46G~K

vs=25~35m/s

Table speed vw=10~30m/min (rectangular table)

Vertical feed fr=0.005~0.05mm/stroke

Rough grinding: fr=0.02~0.05mm

Finish grinding: fr=0.005~0.015mm

Spark-out grinding: 2~3 passes with no feed

【Surface Grinding Accuracy】

Parallelism 0.005~0.02mm/300mm

Flatness 0.005~0.02mm/300mm

Ra0.4~1.6μm

【Surface Grinding Problems】

1. Workpiece warping

Cause: thermal deformation of thin parts

Countermeasure: reduce the grinding depth / adequate cooling / grind both sides

2. Surface burning

Cause: insufficient cooling

Countermeasure: adequate cooling / a soft wheel

3. Parallelism error

Cause: a dirty table surface / magnetic chuck

Countermeasure: clean the table / dress the chuck

【Grinding Thin Parts】

1. Reduce the grinding depth (0.005mm)

2. Grind both sides repeatedly (eliminates the warping)

3. Adequate cooling

4. Use a low hardness wheel

5. Increase the number of spark-out passes

6. Use a vacuum chuck / low melting point alloy fixture if required

Centerless Grinding and Form Grinding

【Principle of Centerless Grinding】

The workpiece is not supported between centers

It is supported by the work rest and the guide wheel

The grinding wheel cuts while the guide wheel rotates the workpiece

【Three Methods】

1. Through-feed method (longitudinal grinding)

The guide wheel is tilted α=1~5°

The workpiece passes through automatically (axial feed)

Suited to smooth cylindrical pins / shafts

High productivity

2. Infeed method

The workpiece is positioned axially

The guide wheel rotates it while the wheel feeds in

Suited to stepped shafts / form parts

3. Combined method

Through-feed + infeed

Suited to complex parts

【Centerless Grinding Parameters】

Wheel speed vs=25~35m/s

Guide wheel speed vr=15~30m/min (the workpiece speed)

Guide wheel tilt α=1~5° (through-feed)

Large α → fast feed, lower accuracy

Small α → slow feed, high accuracy

Axial feed speed:

va = π·Dg·ng·sinα/1000 (m/min)

Dg — the guide wheel diameter

ng — the guide wheel speed

【Characteristics of Centerless Grinding】

Advantages:

① No centers needed, easy loading and unloading

② Continuous machining, high efficiency

③ The workpiece does not bend or deform

④ Easy to automate

Disadvantages:

① The coaxiality cannot be guaranteed (there is no locating datum)

② Long stepped shafts cannot be ground

③ Non-circular surfaces cannot be ground

④ The setup is complicated

【Accuracy】

Dimensional accuracy IT6~IT7

Roundness 0.5~2μm (0.1μm is achievable)

Cylindricity 1~3μm

Ra0.4~0.8μm

【Applications】

Pins / piston pins / rollers / bearing raceways

Short small diameter shafts

Suited to large batch production

【Form Grinding】

Complex shapes are ground with a form wheel

Wheel dressing methods:

1. Diamond pen dressing (simple shapes)

2. Roll dressing (complex shapes, a roller)

3. CNC dressing (a CNC wheel dresser)

4. Electroplated wheels (pre-formed, cannot be dressed)

【Form Grinding Applications】

1. Gear tooth form grinding

Butterfly wheels / tapered wheels

Generating method (0° method / 15° method)

Forming method (a directly formed wheel)

2. Spline grinding

A form wheel grinds the spline flanks and the root diameter

3. Thread grinding

Single wheel threads (finish grinding)

Multi-wheel threads (rough grinding, high efficiency)

4. Cam grinding

With a template / CNC

5. Mould cavity grinding

A form wheel with a coordinate grinder

6. Machine tool guideway grinding

A wide wheel with form dressing

【Form Grinding Accuracy】

Gear tooth form accuracy DIN grade 4~6

Tooth flank Ra0.4~0.8

Thread accuracy 4H~6H

【Precautions for Form Grinding】

1. Wheel dressing is the key

2. Wheel wear affects the shape (compensation is needed)

3. Adequate cutting fluid

4. Avoid burning

5. Multiple finishing passes (reduce the error)

Grinding Burns and Grinding Cracks

【Grinding Burns】

The high temperature in the grinding zone (>500℃) changes the structure of the workpiece surface

Types:

1. Temper burn

Temperature >Ac1 (727℃) → pearlite → austenite → slow cooling to sorbite

The hardness drops

2. Re-hardening burn

Temperature >Ac3 → austenite → rapid cooling to martensite

Secondary hardening, the hardness rises but it becomes brittle

It is surrounded by a tempered softened zone

3. Tempered burn

Temperature <Ac1 (727℃) → martensite → tempered troostite / sorbite

The hardness drops

【Identifying Burns】

1. The surface colour (the oxide film)

400℃: pale yellow

500℃: yellow brown

600℃: purple

700℃: blue

2. The acid etching method

The burnt area has a different colour

3. Micro hardness

The hardness changes in the burnt area

4. Metallography

The structure changes

【Grinding Cracks】

A network of cracks appears on the surface of a hardened part after grinding

Causes:

① The grinding heat + the residual stress

② The workpiece was not tempered enough

③ A high grinding temperature

Features:

① Network / parallel cracks

② A depth of 0.1~0.5mm

③ Perpendicular to the grinding direction

④ Common on hardened parts

【Preventing Burns and Cracks】

1. Reduce the grinding heat

- A soft wheel (self sharpening)

- A coarse grit (good heat dissipation)

- A lower wheel speed

- Reduce the grinding depth

- Adequate cooling (high pressure / high flow)

2. Pretreat the workpiece

- Temper fully (removes the stress)

- Cryogenic treatment of the workpiece (stabilises the structure)

- Eliminate the network carbides

3. Process measures

- Separate the roughing and the finishing

- Several passes (a small depth of cut each time)

- Spark-out grinding (no spark grinding)

- Adequate cutting fluid

4. Wheel selection

- A soft wheel (G/H)

- Large pores (heat dissipation)

- A coarse grit (36~46)

【Grinding Fluid】

1. Emulsion (good cooling)

2. Extreme pressure cutting oil (good lubrication)

3. Synthetic fluid (general purpose)

Flow: >10L/min

High pressure: 1~5MPa (directed straight into the grinding zone)

Filtration: <10μm (prevents the wheel from clogging)

【Inspecting Grinding Burns】

1. Acid etching (5% nitric acid alcohol)

2. Observe the surface colour with the naked eye

3. Micro hardness

4. Metallographic structure

5. Magnetic particle inspection (cracks)

Honing and Lapping Precision Processes

【Honing】

Purpose: improve the bore accuracy and the surface quality

Accuracy: IT6~IT7

Roughness: Ra0.1~0.8

Roundness: 1~3μm

Principle:

The honing head (several stones) rotates and reciprocates inside the bore

A cross hatch pattern is produced

Characteristics:

① A small machining allowance (0.02~0.1mm)

② It corrects the bore form error

③ It improves the surface quality (the cross pattern retains oil)

④ It cannot correct the position error

Applications:

- Engine cylinder bores

- Hydraulic cylinder bores

- Spindle bores

- Connecting rod big end bores

【Honing Parameters】

The honing speed v (combined):

v circumferential + v reciprocating

v = √(v1²+v2²)

v1=15~30m/min (circumferential)

v2=5~15m/min (reciprocating)

Crossing angle: 30~60° (45° is common)

Stones:

Abrasive: WA / GC / CBN

Grit: 120~600

Hardness: J~L

Pressure:

Rough honing: 0.5~2MPa

Finish honing: 0.2~0.8MPa

Coolant: kerosene / kerosene + castor oil

【Lapping】

Purpose: the highest accuracy and surface quality

Accuracy: IT5~IT6

Roughness: Ra0.012~0.1

Principle:

The workpiece + the lap + the abrasive + the lapping fluid

Driven by hand or by a machine

The abrasive rolls and slides to remove the material

Characteristics:

① Extremely high accuracy

② Excellent surface quality

③ Almost no heat is generated (no burning)

④ Limited correction of the form error

⑤ Slow

【Types of Lapping】

1. Wet lapping

Abrasive + liquid

Cutting dominated

Ra0.1~0.4

2. Dry lapping

The abrasive is pressed into the lap and then lapped

Squeezing dominated

Ra0.012~0.1

A mirror finish

3. Polishing

A soft polishing wheel + polishing compound

Ra0.012~0.8

It does not improve the accuracy

【Lapping Parameters】

Abrasive:

Rough lapping: W14~W28

Finish lapping: W5~W14

Super fine lapping: W1~W5

Lapping fluid: kerosene + engine oil + stearic acid

Pressure: 0.05~0.3MPa

Speed: 20~100m/min

【Lapping Applications】

1. Gauge blocks (the datum)

2. Precision gauges

3. Matched pairs for high pressure pumps

4. Valve spools and bushes

5. Optical parts

6. Semiconductor wafers

【Super Finishing】

Purpose: improve the surface quality (without correcting the form error)

Ra: 0.012~0.1

Principle:

The stone lightly presses the workpiece, with vibration + rotation

A low frequency vibration (10~30Hz)

Characteristics:

① No heat is generated

② Surface compressive stress (favourable for fatigue)

③ It improves the contact accuracy

④ It is more efficient than lapping

Applications: bearing raceways / crank journals / cams

High Speed Grinding and Creep Feed Grinding

【High Speed Grinding (HSG)】

Wheel speed vs=60~120m/s (ordinary 30~35)

Advantages:

① The chip of a single grain is thin → small grinding forces

② A high wheel peripheral speed → the grinding temperature is actually lower (the heat is carried away by the chips)

③ The efficiency improves by 3~10 times

④ A long wheel life

⑤ Good surface quality

Requirements:

① A high speed wheel (a high strength bond)

② A high speed spindle (>6000rpm)

③ High power (the grinding power is high)

④ Strict safety protection (the wheel may burst)

⑤ Adequate cooling (high pressure)

Applications:

Automotive crankshafts / camshafts

Bearing raceways

Gear tooth flanks

【Creep Feed Grinding (CFFG)】

A deep depth of cut with a slow feed

ap=1~30mm (cuts to the full depth in one pass)

vf=0.1~10mm/min (very slow)

Advantages:

① Formed in one pass (grooves / profiles)

② An even distribution of the grinding forces

③ A long wheel life

④ Good surface quality

Disadvantages:

① A large amount of grinding heat (a long contact arc)

② High pressure cooling is required

③ Expensive equipment

Applications:

Turbine blade fir tree roots (formed in one pass)

Gear tooth forms

Grooves / collet slots

Machine tool guideways

【Continuous Dress Creep Feed (CDCF)】

The wheel is dressed while grinding

The wheel stays sharp

It improves the accuracy and the surface quality

Parameters:

vs=30~60m/s

ap=0.5~5mm

vf=5~50mm/min

The dressing speed 0.1~0.5mm/min (continuous)

【High Efficiency Deep Grinding (HEDG)】

vs=100~200m/s

ap=1~10mm

vf=500~10000mm/min

Combines high speed grinding with deep grinding

An extremely high efficiency

A metal removal rate >1000mm³/s

【Grinding Fluid (High Speed / Deep Grinding)】

1. A large flow rate (50~200L/min)

2. A high pressure (3~15MPa)

3. The flow velocity matches the wheel (>30m/s)

4. Filtration (<5μm)

5. Temperature control (±1℃)

【Safety Precautions】

1. The wheel speed matches the rating (it must not be exceeded)

2. The guard is robust

3. Balancing (the G2.5 grade)

4. A trial run (idle for 5min)

5. Stand clear of the direction the wheel would burst in

6. The coolant spray direction is correct

Evaluation of the Grinding Surface Integrity

【Definition of Grinding Surface Integrity】

The state of the surface layer (physical / chemical / mechanical)

It includes:

1. The surface topography (roughness / waviness)

2. The surface defects (cracks / burns)

3. The physical and mechanical properties (hardness / residual stress)

4. The metallographic structure

【Characteristics of the Surface Layer】

After grinding the surface is divided into:

1. The contamination layer (the outermost, embedded abrasive / oxidation)

2. The plastic deformation layer (work hardening)

3. The phase transformation layer (quenched / tempered)

4. The affected base material (the residual stress field)

The total affected depth: 0.05~0.5mm

【Surface Roughness】

Ordinary grinding: Ra0.8~1.6

Finish grinding: Ra0.4~0.8

Precision grinding: Ra0.1~0.4

Mirror grinding: Ra<0.025

Factors influencing it:

1. The wheel grit (finer → a lower Ra)

2. The wheel speed (higher → a lower Ra)

3. The workpiece speed (lower → a lower Ra)

4. The feed (smaller → a lower Ra)

5. The wheel dressing (sharp → a lower Ra)

6. The cutting fluid (adequate → a lower Ra)

7. The machine rigidity (higher → a lower Ra)

【Surface Waviness】

Periodic waviness

Causes:

1. The wheel is out of balance

2. The spindle vibration

3. The workpiece vibration

Measurement: a roundness tester / a profilometer

【Changes in the Micro Hardness】

1. Grinding softening (tempering)

A temperature below Ac1 → the martensite is tempered

The hardness drops

2. Grinding hardening (secondary quenching)

A temperature above Ac3 with rapid cooling

Austenite → martensite

The hardness rises (it becomes brittle)

It is surrounded by a softened zone

3. Work hardening

Plastic deformation

The dislocation density increases

The hardness rises

【Residual Stress】

The ground surface is normally in tension

Cause: thermo-plastic deformation (it contracts on cooling after heating and is constrained)

Adverse effects:

① The fatigue strength drops

② Stress corrosion cracking

③ Deformation

Improvement measures:

① Reduce the grinding heat (a soft wheel / adequate cooling)

② Shot peening / roller burnishing (it converts it to a compressive stress)

③ Ageing treatment

【Changes in the Metallographic Structure】

1. The tempered structure (sorbite / troostite)

2. The secondary quenched martensite

3. The decarburised layer (high temperature oxidation)

4. The grinding lines

【Inspection Methods】

1. The surface topography

- A roughness tester

- An optical microscope

- SEM

2. The micro hardness

- A Vickers micro hardness tester

- The distribution along the depth

3. The residual stress

- X-ray diffraction (non destructive)

- The hole drilling method (semi destructive)

- Ultrasonic (non destructive)

4. The metallographic structure

- Sectioning + polishing + etching

- An optical / an electron microscope

5. The defect inspection

- Magnetic particle inspection (ferromagnetic)

- Penetrant inspection (any material)

- Eddy current (conductive)

- Acid etching (burns)

【Quality Grades (Critical Parts)】

1. Aerospace parts

- No burns allowed

- The residual stress is controlled

- 100% inspection

2. Moulds

- No burns allowed

- Polished to Ra<0.1

3. Gauges

- Dimensional stability

- Ageing treatment

- Low residual stress

4. Rolling bearings

- Surface compressive stress (favourable for fatigue)

- A high hardness

- No burns

Grinding Wheel Dressing Technology

【Purpose of Wheel Dressing】

1. Restore the geometry of the wheel

It goes out of round after wear

Dressing restores the cylindricity

2. Restore the sharpness of the wheel

The grains become blunt / clogged

Dressing exposes new grains

3. Dress the wheel to a form

Grinding a form surface (a thread / a tooth form)

The wheel is dressed to the corresponding shape

【Dressing Tools】

1. A diamond pen (single point)

The most common

A large grain natural / synthetic diamond

Suited to ordinary wheels

2. A diamond dresser

Several sintered diamonds

A long life

Suited to large wheels

3. A diamond roller (form dressing)

The roller shape = the workpiece shape

It dresses the form in one operation

Suited to large batches

4. A diamond dish dresser

It dresses the angle

Suited to dressing the wheel angles

5. A silicon carbide wheel against a wheel

Wheel against wheel dressing

Economical

6. A steel roller (no diamond)

Roller burnishing dressing

Suited to soft wheels

【Dressing Parameters】

1. The dressing depth ad

Rough dressing: 0.02~0.05mm/stroke

Finish dressing: 0.005~0.02mm/stroke

The total dressing depth: 0.05~0.2mm

2. The dressing feed fd

Rough dressing: 0.3~0.5mm/rev (per wheel revolution)

Finish dressing: 0.05~0.2mm/rev

A slow finish dressing → a smooth wheel surface → a low Ra on the workpiece

A fast rough dressing → a rough wheel surface → small grinding forces

3. The number of dressing passes

2~3 rough passes (remove the worn layer)

1~2 finish passes (polish)

1~2 spark-out passes with no feed

4. The dressing direction

Traverse (the same direction as the wheel rotation)

Reverse (the opposite) — sharper

Traverse is normally used

【Dressing and the Grinding Quality】

A rough dressed wheel:

The grains stand high, a large chip pocket

Small grinding forces, a high metal removal rate

A higher Ra on the workpiece (1.6~3.2)

A finely dressed wheel:

The grains are level, many micro edges

Large grinding forces, a low metal removal rate

A low Ra on the workpiece (0.4~0.8)

Super finishing (mirror grinding):

An extremely slow feed + many spark-out passes

Micro edge cutting + friction polishing

Ra<0.1

【Form Dressing】

1. A single point diamond dressing a form surface

A CNC dresser

It follows the shape path

Suited to small batches

2. Diamond roller dressing

The roller shape = the workpiece shape

The roller rotates opposite to the wheel

It forms the shape in one cut

Suited to large batches

The roller is expensive but it has a long life

3. A steel roller + a diamond dressing

The steel roller forms it first

Then the diamond gives a finish pass

【Precautions for Dressing】

1. Cool adequately (dressing generates heat)

2. Aim the diamond pen tip at the wheel center

3. Tilt it 5~10° (avoids grooves at the tip)

4. Balance the wheel after dressing (if necessary)

5. Run the wheel idle for 1~2min after dressing (removes the loose grains)

6. The dressing frequency (depends on the wheel wear)

【Judging the Wheel Wear】

1. Burning on the workpiece surface

2. Chatter marks on the workpiece

3. An increase in the grinding force

4. A change in the grinding noise

5. Unstable dimensions

6. The surface roughness deteriorates

【Dressing Cycle】

Ordinary grinding: 1~2 times per shift

Precision grinding: every part or every few parts

High volume: by the piece count

Automated grinding: automatic dressing + compensation

Related quick references: Machining FundamentalsCutting Tool MaterialsTool GeometryTurning ProcessMilling ProcessDrilling ProcessBoring ProcessMachining AllowanceProcess SequencingTypical ProcessesCNC ProgrammingFixture DesignSpecial Machining Processes

Related 3D models: Ready to build it? Download free 3D models & CAD drawings at MOULDL »