Pitfall: inside bend radius R<sheet thickness (low-carbon steel) or R<2× sheet thickness (stainless steel)
Consequence: cracking on the outer surface / failed bending
Correct practice: low-carbon steel R≥t, stainless steel R≥2t, aluminum alloy R≥1.5t
Pitfall: bend edge distance (from bend line to edge) <3× sheet thickness
Consequence: the edge stretches and tears during bending
Correct practice: bend edge distance ≥3t (≥5t preferred)
Pitfall: spacing between adjacent blanks <2× sheet thickness
Consequence: material deformation during blanking / large burrs / short die life
Correct practice: spacing ≥2t (≥3t preferred)
Pitfall: no relief notch (crack-stop groove) where sheet-metal bends meet
Consequence: tearing where the bends meet
Correct practice: cut a relief notch with R≥1mm where the bends meet
Pitfall: stiffening rib depth <3× sheet thickness
Consequence: insufficient stiffening (a too-shallow rib is nearly as good as no rib)
Correct practice: stiffening rib depth ≥5t (≥10t recommended)
Pitfall: weld nuts on the sheet metal without a locating hole / locating dimple
Consequence: the nut is mispositioned → bolt assembly becomes difficult
Correct practice: provide a punched locating hole or a locating boss where the nut is welded
Pitfall: no flange on the edge of a large sheet-metal opening
Consequence: insufficient edge strength / easy to cut hands
Correct practice: flange the edge of holes or openings (height ≥3t)