Design Pitfalls · Heat Treatment (Quick Reference)

Common Heat Treatment Process Problems

① Pitfall: An abrupt section change on a quenched part has no transition fillet

Correct practice: Use a large-radius transition at the section change

② Pitfall: Sharp corners on quenched parts are not chamfered

Correct practice: Chamfer or round all sharp corners

③ Pitfall: An asymmetric workpiece is quenched directly

Correct practice: Tie it up or pre-deform to compensate

④ Pitfall: No tempering after quenching, or tempering is delayed

Correct practice: Temper within 4 hours after quenching

⑤ Pitfall: Temper embrittlement is ignored

Correct practice: Rapidly cool alloy steels such as 40Cr after tempering

⑥ Pitfall: The case depth of a carburized part is too deep

Correct practice: Select the depth by service condition: 0.5~1.5mm

⑦ Pitfall: A large workpiece is immersed incorrectly during quenching

Correct practice: Immerse vertically to reduce thermal stress

Insufficient Oil Cooling for Large Sections

Pitfall: A large-section part (>50mm) is quenched relying on oil cooling alone

Consequence: Insufficient core hardness / incomplete hardening

Correct: 45 steel <30mm water quench / 30~50mm water-oil double medium quench

No Tempering After Quenching

Pitfall: The part is not tempered immediately after quenching (left standing >24h)

Consequence: High quenching stress → cracking

Correct: Temper immediately within 2h of quenching / stress relief

No Anti-Carburizing Masking on Carburized Parts

Pitfall: Areas of a carburized part that must not be carburized have no anti-carburizing protection

Consequence: Threads and similar areas are also carburized → high brittleness

Correct: Apply an anti-carburizing agent (borax + copper oxide) / leave machining allowance and remove it afterward

Rust or Oil on the Part Before Nitriding

Pitfall: The part surface is not clean before nitriding (rust or oil present)

Consequence: Uneven nitride layer / local areas fail to nitride

Correct: Thoroughly clean, de-rust and dry before nitriding

No Chamfer on Sharp Corners of Quenched Parts

Sharp corners and edges of quenched parts should be chamfered R≥2mm / without a chamfer → stress concentration at the corner → quenching cracks / the larger the section, the more necessary it is

Wrong Quenching Medium for Large Sections

45 steel parts with a section >30mm should be water quenched, and >50mm oil quenched / otherwise hardness is insufficient / use double-medium quenching (water quench then oil cool) or choose a steel with better hardenability such as 40Cr

Tempering Not Done Promptly After Quenching

Temper within 2h after quenching / if delayed → quenching stress is released → cracking / large parts may even crack within minutes of quenching

Soaking in the Temper Embrittlement Zone

When tempering steels such as 38CrMoAl or 45CrNi, avoid the 450~650℃ temper embrittlement zone / cool rapidly (water quench / oil quench)

Case Depth Too Deep

A case depth >1.5mm (for general parts) means too long a carburizing time, low efficiency and high cost / select the depth by load / normally 0.5~1.2mm

Threads on Carburized Parts Not Protected

Thread holes and non-carburized surfaces on carburized parts must be coated with an anti-carburizing agent / otherwise the threads are also carburized → high brittleness / thread stripping / apply an anti-carburizing agent or leave machining allowance

Nitride Layer Too Thin

A nitride layer <0.2mm gives insufficient wear resistance / it should be ≥0.3mm (gas nitriding) / raise the nitriding temperature or extend the nitriding time

Insufficient Allowance for Heat Treatment Distortion

Heat treatment distortion: shafts 0.1~0.3mm, plates 0.2~0.5mm / without allowance the part is scrapped after distortion / leave grinding allowance / leave 0.5~1mm on quenched and tempered parts

Uneven Hardened Layer in Induction Hardening

In induction hardening, an uneven gap between the inductor and the workpiece produces an uneven hardened depth / keep the gap uniform (1~3mm)

Improper Solution and Aging of Aluminum Alloys

After solution treatment, aluminum alloy parts should be quenched as quickly as possible (transfer ≤15s) / if delayed → the supersaturated solid solution decomposes → strength drops / control the aging temperature strictly by temper designation

Water Quenching of Alloy Steel

Alloy steel (40Cr / 42CrMo) is normally oil quenched / water quenching carries a high cracking risk / simple shapes may be water quenched (water temperature ≤150℃, temper immediately)

Core Hardness of Carburized Parts Too High

A core hardness >HRC45 gives insufficient toughness → brittle fracture / core hardness depends on the hardenability of the material and the quenching temperature / control 20CrMnTi core to HRC35~45

Nitriding Layer Too Brittle and Hard to Grind

The nitride layer is brittle (white layer) and is not suitable for grinding / where a dimensional requirement exists, allow 0.02~0.05mm before nitriding / nitride directly to size

No Tempering After Quenching Spring Steel

Spring steel (65Mn / 60Si2MnA) must be tempered immediately after quenching (380~480℃) / without tempering → high brittleness / it breaks under the first load

Case Depth Not Meeting the Drawing

The case depth of a carburized part should be inspected (metallographic method / hardness method) / if it does not conform → rework or scrap / depth tolerance ±0.1mm

Straightening Not Done While Hot After Quenching

A quenched part should be straightened while still hot, before tempering / straightening after cooling → high stress → fracture / straighten long shafts within 4h of quenching

Induction Hardening Along the Tooth Space on Small Gears

Small gears (m<3) should be induction hardened tooth by tooth, along the tooth space / hardening the whole tooth → the tooth tip overheats → uneven tooth flank hardness

Unclear Hardness Specification for Heat Treated Parts

【Unclear Hardness Specification for Heat Treated Parts】Heat treatment hardness should be specified as HRC (Rockwell) or HB (Brinell) / if not specified → it cannot be judged during inspection / specify a hardness range for critical parts (e.g. HRC48~53)

Hardened Layer Depth Not Specified

【Hardened Layer Depth Not Specified】Carburized, nitrided and induction hardened parts should specify the hardened layer depth / if not specified → it cannot be inspected / too shallow → insufficient wear resistance / too deep → high brittleness

Excessive Hardness Range on Quenched Parts

Design pitfall: an excessive hardness range on quenched parts (e.g. HRC40~55) makes heat treatment hard to control / unify the range or split it into two grades

Workpiece Not Cleaned Promptly After Quenching

The workpiece should be cleaned promptly after quenching (degrease / remove salt) / if not, the surface rusts and the next operation has to be redone

Uneven Hardened Layer on Induction Hardened Parts

An uneven gap between the inductor and the workpiece gives an uneven hardened depth / adjust the inductor position / rotate the workpiece

No Machining Allowance Left on Quenched and Tempered Parts

After quenching and tempering the part has an oxide scale and is distorted / leave a machining allowance (1~2mm for parts ≤50mm, 2~3mm above 50mm)

No Hardened Layer Depth on Induction Hardened Parts

【No Hardened Layer Depth on Induction Hardened Parts】Induction hardened parts should specify the hardened layer depth (0.5~2mm) / without it → it cannot be inspected → hardness is insufficient or too hard and brittle

Carburizing Without Distinguishing Areas

【Carburizing Without Distinguishing Areas】Different areas of a carburized part should have different hardness requirements / use anti-carburizing agent to differentiate / carburizing everything makes one spot hard and brittle → fracture

Finish Machining Before Stress Relief

【Finish Machining Before Stress Relief】Quenched and tempered parts should be rough machined first, then stress relieved and tempered, and finish machined afterwards / finishing directly → the stress is released after machining → distortion

Mold Not Tempered Promptly After Quenching

A mold should be tempered within 1h of quenching / a delay carries a high risk of cracking / large molds may even crack within minutes of quenching

Post-Weld Heat Treatment Delayed Beyond the Specified Time

Post-weld heat treatment should be carried out within 48h of welding / a delay → cold cracks → preheating is needed again before the treatment can proceed

Hardness Not Checked After Quenching

Quenched parts should be hardness checked piece by piece / without checking, non-conforming hardness passes into the next operation

Related quick references: Welding PitfallsCasting PitfallsShafting PitfallsSheet Metal PitfallsAssembly PitfallsHydraulic PitfallsPneumatic PitfallsShafting DesignHousing DesignWelded StructuresSheet Metal StructuresSpring DesignBolt ConnectionsBearing Arrangement

Related 3D models: Ready to build it? Download free 3D models & CAD drawings at MOULDL »