C: 0.42~0.50%
Si: 0.17~0.37%
Mn: 0.50~0.80%
Tensile strength σb: ≥600 MPa
Yield strength σs: ≥355 MPa
Elongation δ: ≥16%
Reduction of area ψ: ≥40%
Impact energy Akv: ≥39 J
Hardness: HB 220~250
Normalizing: 840~860℃ air cooling, HB 170~217
Quenching: 820~840℃ water cooling
High-temperature tempering (quenched and tempered): 550~650℃, HB 220~250
Shafts, gears, keys, bolts, connecting rods and other general load-bearing parts
Not suitable for large sections (>60mm, insufficient core hardness)
Good machinability in the normalized condition
Average weldability, preheat before welding
C: 0.37~0.44%
Cr: 0.80~1.10%
Tensile strength σb: ≥800 MPa
Yield strength σs: ≥650 MPa
Elongation δ: ≥12%
Reduction of area ψ: ≥45%
Impact energy Akv: ≥47 J
Hardness: HB 240~280
Quenching: 840~860℃ oil cooling
Tempering: 520~560℃, HB 240~280
Critical shafts, gears, connecting rods, bolts, spindles
Can be hardened through within 100mm diameter
Susceptible to temper embrittlement (450~650℃); rapid cooling after tempering is essential
Poor weldability; preheat before welding and post-weld heat treatment
Surface hardening may be applied for further wear resistance
Q — yield strength
235 — yield strength ≥235MPa
Q235A: no impact test
Q235B: 20℃ impact test
Q235C: 0℃ impact test
Q235D: -20℃ impact test
Yield strength: ≥235MPa (thickness ≤16mm)
Tensile strength: 370~500MPa
Elongation: ≥26%
Welded structures, sections, brackets, frames, unimportant structural parts
Low cost, good weldability, easy to machine
Relatively low strength, not suitable for heavily loaded parts
Not strengthened by heat treatment
Equipment frames, bases, guardrails, handrails
Welded parts, sheet metal parts, general structural parts
C: ≤0.07%
Cr: 17.0~19.0%
Ni: 8.0~11.0%
Tensile strength σb: ≥520 MPa
Yield strength σs: ≥205 MPa
Elongation δ: ≥40%
Hardness: HB≤187
① Good corrosion resistance (atmosphere / water / weak acids and alkalis)
② Non-magnetic
③ Excellent low-temperature toughness
④ Cannot be strengthened by heat treatment (cold work hardening only)
⑤ Severe work hardening, poor machinability
Food machinery, chemical equipment, medical devices
Precision instruments, decorative parts
Use carbide cutting tools when machining
Control the heat input when welding
Large springback when cold bending
Related quick references: Heat Treatment Process ParametersCarbon Structural SteelQuality Carbon SteelAlloy Structural SteelBearing SteelTool SteelStainless SteelCast IronAluminium AlloyNon-ferrous AlloysHeat Treatment ProcessesCommon SteelsCast Iron & Non-ferrous Metals