Materials & Heat Treatment · Heat Treatment Processes (Quick Reference)

Quenched and Tempered Process Parameters

【Quenched and Tempered Treatment】A dual heat treatment process of quenching followed by high-temperature tempering.

【Purpose】

Obtain a tempered sorbite structure

Achieve good overall mechanical properties (high strength + high toughness)

【Process Parameters】

45 steel:

Quenching temperature: 820~840℃

Quenching medium: water

Tempering temperature: 550~650℃

Hardness after tempering: HB 200~250

40Cr:

Quenching temperature: 840~860℃

Quenching medium: oil

Tempering temperature: 520~560℃

Hardness after tempering: HB 240~280

35CrMo:

Quenching temperature: 850~870℃

Quenching medium: oil

Tempering temperature: 500~560℃

Hardness after tempering: HB 260~300

42CrMo:

Quenching temperature: 840~860℃

Quenching medium: oil

Tempering temperature: 540~640℃

Hardness after tempering: HB 240~300

【Cautions】

① The higher the tempering temperature, the lower the hardness and the higher the toughness

② Temper immediately after quenching (within 4 hours)

③ Allow 1 min/mm of tempering holding time

④ Extend the holding time appropriately for large-section parts

【Relation Between Tempering Temperature and Hardness (45 Steel)】

550℃→HB 240~250

600℃→HB 220~230

650℃→HB 200~210

Carburizing and Quenching Process Parameters

【Carburizing and Quenching】Carburizing the surface of low-carbon steel and then quenching.

【Purpose】

High surface hardness (HRC 58~63) + high core toughness

Suitable for heavy-duty gears and transmission shafts

【Common Materials】

20CrMnTi, 20CrMo, 20CrNiMo

【Process Parameters】

Carburizing temperature: 900~950℃

Carburizing medium: kerosene / methanol / natural gas

Carburizing time: according to the required case depth (about 0.15~0.2mm/h)

【Case Depth Selection】

Light-duty gears: 0.3~0.6mm

Medium-duty gears: 0.6~1.0mm

Heavy-duty gears: 1.0~1.5mm

Extra heavy-duty: 1.5~2.0mm

【Quenching Process】

Direct quenching: after carburizing, cool to 820~850℃ and quench directly in oil

Single quench: after carburizing, air cool, then reheat and quench

【Tempering】

Low-temperature tempering: 180~200℃

Hardness after tempering: HRC 58~63

【Quality Inspection】

① Case depth (metallographic or hardness method)

② Surface hardness

③ Core hardness (HRC 30~42 is preferred)

④ Metallographic structure (martensite grade)

⑤ Effective hardened layer depth

Hardness Conversion Table (HB/HRC/HV)

【Common Hardness Conversion Table】

Brinell HB | Rockwell HRC | Vickers HV | Tensile strength σb (MPa)

-----------------------------------------------------

600 | 57 | 620 | 2000

550 | 54 | 570 | 1850

500 | 50 | 520 | 1700

450 | 46 | 470 | 1500

400 | 41 | 410 | 1350

350 | 36 | 360 | 1150

300 | 31 | 310 | 1000

250 | 24 | 260 | 830

220 | 20 | 230 | 750

200 | 15 | 210 | 680

180 | 10 | 190 | 620

160 | - | 170 | 550

140 | - | 150 | 480

【Notes on Conversion】

① The above are approximate values for steel; they vary slightly by material

② Below HRC 20 it is more accurate to use HB

③ Conversion is relatively reliable in the HRC 20~70 range

④ HV suits thin hardened layers

⑤ HRC is common for quenched steels; HB is common for annealed / normalized / quenched-and-tempered parts

【Selection Advice】

HB: annealed / normalized / quenched-and-tempered parts (HB<300)

HRC: quenched parts / carburized parts (HRC 20~65)

HV: nitrided layers / chrome plated layers (thin layers)

HS: large castings and forgings (Shore hardness)

【Related Modules】FT_08_Hardness Conversion Calculator

Related quick references: Heat Treatment Process ParametersCarbon Structural SteelQuality Carbon SteelAlloy Structural SteelBearing SteelTool SteelStainless SteelCast IronAluminium AlloySteelsNon-ferrous AlloysCommon SteelsCast Iron & Non-ferrous Metals

Related 3D models: Ready to build it? Download free 3D models & CAD drawings at MOULDL »
MOULDL · Mechanical Engineering Knowledge Base · free self-study reference for machine designers, 3D CAD models at MOULDL