F=L×t×τ_b
L blanking contour perimeter (mm), t material thickness (mm)
τ_b shear strength (MPa), generally taken as (0.6~0.8)× the tensile strength
F_d=K_d×F, K_d=0.02~0.08
F_t=K_t×F×n, K_t=0.03~0.07, n is the number of parts stuck in the die
Required total force F_total=F+F_d+F_t
Press tonnage ≥1.3×F_total
Recommended clearance: 8%~12%t for mild steel, 12%~18%t for hard steel
r_min/t (t is the sheet thickness):
Mild steel: r_min=0.5t at 90° bending, carbon steel Q235: r_min=1.0t
Stainless steel 304: r_min=2.0t, aluminium alloy: r_min=2.0t
Springback angle Δα=α×r×σ_s/(E×t)
α bending angle, r bending radius, σ_s yield strength
① Negative springback compensation (the die angle is 2°~5° smaller than required)
② Add a coining operation (calibration)
③ High-frequency heating bending
m=d/D, d is the diameter after drawing, D is the blank diameter
m1 (first draw)=0.50~0.60 (carbon steel)
m2 (second draw)=0.75~0.82
mn (subsequent)=0.78~0.85
F_Q=A×q, A is the blank holder area, q is the unit blank holding force (2~4MPa)
Use a blank holder (when the drawing ratio m is below the m1 limit)
Increase the number of draws, increase the material thickness, use draw beads
Drawing requires a dedicated drawing lubricant, maintaining an oil film of 0.01~0.02mm