718H (equivalent to P20+Ni): hardness HRC30~36, machined directly in the pre-hardened condition
Applications: high volume injection moulds (below 1,000,000 shots)
NAK80: hardness HRC37~43, pre-hardened, good mirror polishability
Applications: transparent part / mirror finish moulds
SKD61 (8407/H13): quenched to HRC48~52
Applications: high wear moulds / sliders / lifters
S136 (stainless): quenched to HRC48~52
Applications: corrosion resistant / high gloss / transparent parts
General parts: 718H offers the best value for money
Transparent or mirror parts: NAK80 or S136
High wear parts: quenched SKD61
High corrosion (PVC): S136
Pre-hardened HRC30~36, generally not heat treated
If nitriding is required: 520℃×8~12h, nitrided layer 0.15~0.25mm
Pre-hardened HRC37~43, generally not heat treated
Quenching temperature: 1020~1050℃, air cool or gas quench
First temper: 560~580℃×2h
Second temper: 550~570℃×2h
Final hardness: HRC48~52
Quenching temperature: 1000~1040℃, oil cool or gas quench
Tempering temperature: 180~250℃ (low temperature temper, high hardness)
Or 500~550℃ (high temperature temper, high toughness)
Final hardness: HRC48~55
① Vacuum heat treatment gives the least distortion
② The workpiece must be thoroughly preheated before quenching (two stages at 650℃/850℃)
③ At least two tempers are required