Product Design · Die Casting Process (Quick Reference)

Die Casting Mould Gating System Design

【Runner (Ingate) Area Calculation】

A_g=G/(ρ×v_g×t_f)

G casting weight (g), v_g ingate velocity (m/s), t_f filling time (s)

【Filling Time】

Wall thickness 1~2mm: t_f=0.01~0.03s

Wall thickness 2~3mm: t_f=0.02~0.06s

Wall thickness 3~5mm: t_f=0.04~0.10s

【Runner (Cross Channel)】

Cross-section A_r=(3~5)×A_g, the length should be as short as possible

Die Casting Aluminium Alloy Composition and Mechanical Properties

【Common Die Casting Aluminium Alloys】

ADC12(A383): Al-Si-Cu series, good fluidity

Tensile σb≥230MPa, hardness HB≥80

ADC10(A380): tensile σb≥250MPa

【Composition Control】

Si: 9.5%~11.5% (improves fluidity)

Cu: 1.5%~3.5% (improves strength)

Fe: ≤1.0% (excess causes brittleness)

【Heat Treatment】

Die castings generally do not receive T6 heat treatment (internal gas pores expand and blister)

Related quick references: Injection Molding ProcessStamping ProcessSurface TreatmentMold StructureRunner SystemCooling SystemMold MaterialsPlastic MaterialsInjection Molding DefectsMold MachiningHot Runner SystemAutomotive MoldsForging Dies

Related 3D models: Ready to build it? Download free 3D models & CAD drawings at MOULDL »
MOULDL · Mechanical Engineering Knowledge Base · free self-study reference for machine designers, 3D CAD models at MOULDL