Knowledge Base › Common Faults › Welding Defects

Common Faults · Welding Defects (Quick Reference Manual)

Welding Hot Crack Defect Analysis

[Phenomenon]

Weld metal cracks along grain boundaries at high temperature, with a zigzag path and an oxidized surface.

[Possible Causes]

① Base metal S / P impurities too high

② Weld depth-to-width ratio too large

③ Cooling rate too fast

④ Improper arc termination; crater not filled

[Diagnostic Method]

① Check base metal and filler S / P content, should be ≤0.04%

② Observe crack morphology (longitudinal / transverse / crater)

③ Use magnetic particle or dye penetrant testing to determine the crack extent

[Corrective Measures]

① Control S / P content in the base metal and filler

② Adjust the groove shape to increase the width-to-depth ratio

③ Preheat 100~150℃ before welding

④ Use current ramp-down or back-burn to fill the crater at arc termination

Welding Cold Crack Defect Analysis

[Phenomenon]

Cracks appear delayed, from hours to days after welding; no oxidation color; intergranular or transgranular.

[Possible Causes]

① High diffusible hydrogen in the weld

② Hardened microstructure in the heat-affected zone

③ High restraint stress in the joint

④ No preheat or insufficient preheat before welding

[Diagnostic Method]

① Use ultrasonic testing to detect internal cracks

② Measure heat-affected zone hardness (should be ≤HV350)

③ Check the preheat temperature records

[Corrective Measures]

① Use low-hydrogen electrodes and dry them strictly (350℃×1h)

② Preheat before welding (by plate thickness: below 20mm 100℃, 20~40mm 150℃)

③ Hydrogen-removal treatment immediately after welding (250~350℃×2h)

④ Keep weld hydrogen content ≤5ml/100g

Welding Porosity Defect Analysis

[Phenomenon]

Round or oval pores appear on or inside the weld, either isolated or densely distributed.

[Possible Causes]

① Shielding gas flow too low (<15L/min) or too high, blowing the shielding away

② Oil, rust, or moisture on the filler wire or base metal surface

(3) Excessive air flow (wind speed > 2 m/s)

④ Insufficient gas purity (CO₂ purity <99.5%)

[Diagnostic Method]

① Visually inspect pore morphology (round pores with smooth inner walls)

② Take X-ray films to determine pore location and size

③ Check the shielding gas flow meter

[Corrective Measures]

① Clean oil and rust from within 20mm on both sides of the groove before welding

② Adjust shielding gas flow (15~25L/min)

③ Set up wind screens

④ Switch to higher-purity gas

⑤ Dry the electrodes strictly

Welding Lack of Fusion Defect Analysis

[Phenomenon]

The weld fails to fuse completely with the base metal or between passes, appearing as strips or patches.

[Possible Causes]

① Welding current too low

② Welding speed too fast

③ Groove angle too small

④ Improper torch angle (not aimed at the fusion face)

[Diagnostic Method]

① Macro metallographic examination of the cross-section

② Ultrasonic testing for lack of fusion

③ Verify the welding procedure parameters

[Corrective Measures]

① Increase welding current appropriately (10~20%)

② Reduce welding speed

③ Increase the groove angle (60°~70°)

④ Adjust the torch angle (10°~15° push angle)

Welding Incomplete Penetration Defect Analysis

[Phenomenon]

The weld root is not fully penetrated, leaving a gap at the root.

[Possible Causes]

① Root face too large (>2mm)

② Root gap too small (<2mm)

③ Welding current too low

④ Back side not gouged before welding the second side

[Diagnostic Method]

① Visually inspect the root

② Use radiographic testing to determine the penetration depth

③ Measure the groove dimensions

[Corrective Measures]

① Keep the root face at 1~2mm

② Root gap ≥2mm

③ Increase welding current

④ Gouge the back side by carbon arc air gouging before welding the second side

Welding Undercut Defect Analysis

[Phenomenon]

The base metal at the weld toe is melted into a groove and not filled with metal.

[Possible Causes]

① Welding current too high

② Welding speed too fast

③ Wire stick-out too long

④ Improper torch angle

[Diagnostic Method]

① Visually inspect the weld toe

② Measure undercut depth and length

[Corrective Measures]

① Reduce welding current

② Slow the welding speed

③ Control wire stick-out (10~15mm)

④ Reduce weave width and increase dwell time at the edges

Welding Overlap Defect Analysis

[Phenomenon]

Molten metal flows onto unfused base metal and piles up into a beaded bump.

[Possible Causes]

① Welding current too high

② Welding speed too slow

③ Wire stick-out too long

④ Unsteady manipulation

[Diagnostic Method]

① Visually inspect the weld appearance

② Measure the overlap size

[Corrective Measures]

① Reduce welding current

② Increase welding speed appropriately

③ Control wire stick-out

④ Improve manipulation consistency

Welding Burn-Through Defect Analysis

[Phenomenon]

Excessive penetration causes the molten pool to collapse and form a hole.

[Possible Causes]

① Welding current too high

② Welding speed too slow

③ Root gap too large

④ No backing when welding thin plate

[Diagnostic Method]

① Visually inspect the burn-through location

② Measure the burn-through hole diameter

[Corrective Measures]

① Reduce welding current (use pulsed welding for thin plate)

② Increase welding speed

③ Reduce the root gap

④ Add a copper or ceramic backing

⑤ For plate thickness <3mm, use low-current CO₂ welding

Welding Crater Crack Defect Analysis

[Phenomenon]

The arc-termination point is not filled; star-shaped cracks form as it cools.

[Possible Causes]

① Current cut off abruptly at arc termination

② Crater not filled

③ Material highly crack-sensitive

[Diagnostic Method]

① Visually inspect the crater area

② Use dye penetrant testing to confirm the crack

[Corrective Measures]

① Use current ramp-down at arc termination

② Fill the crater (back-burn method)

③ Use a crater-fill plate

④ Grind the crater away after arc termination

Welding Poor Bead Formation Defect Analysis

[Phenomenon]

The weld bead is uneven in height and width, with irregular toes.

[Possible Causes]

① Unstable wire feed

② Uneven welding speed

③ Unsteady torch weaving

④ Mains voltage fluctuation

[Diagnostic Method]

① Visually inspect the weld appearance

② Check the wire feed mechanism

[Corrective Measures]

① Check the feed roller pressure and the wire guide tube

② Steady the welding speed

③ Use a track or welding carriage

④ Add a voltage stabilizer

Causes and Prevention of Welding Cracks

[Hot Cracks]

Causes:

① High S / P content in the weld metal

② Excessive welding stress

③ Improper weld shape factor (small width-to-depth ratio)

Preventive measures:

① Control S / P content in the base metal and filler

② Preheat to reduce the cooling rate

③ Select a reasonable groove shape

④ Use low-hydrogen electrodes

[Cold Cracks]

Causes:

① High diffusible hydrogen content

② Hardened microstructure (martensite)

③ High restraint stress

Preventive measures:

① Preheat before welding (per plate thickness and material)

② Slow cooling or post-heating after welding

③ Use low-hydrogen electrodes and dry them

④ Hydrogen-removal treatment immediately after welding

[Solidification Cracks]

Causes:

① Narrow, deep weld

② Crater not filled

Preventive measures:

① Increase the groove angle

② Fill the crater

③ Use current ramp-down at arc termination

Other quick references in this series:Hydraulic systemPneumatic systemMotor electricalEquipment faultsMotor faultsStructural part faultsSensor faultsElectrical faultsQuick diagnosisMechanical component faultsBearing faultsGear faultsHydraulic / pneumatic valves

Related model download:Understood the principle and ready to try?Go to MOULDL to download related 3D models and CAD drawings for free »
MOULDL · Mechanical Engineering Knowledge Base · free self-study reference for machine designers, 3D CAD models at MOULDL